Author: Subject: Anodes for FFC Cambridge Process
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 2-11-2008 at 23:40
Anodes for FFC Cambridge Process


I have been pondering anode materials for the FFC Cambridge Process. Graphite or other forms of carbon are not suitable as they are entirely consumed with release of CO or CO2 as opposed to oxygen. At the process temperature of 900°C, probably no metal would hold up for long.

A document, here, suggests a tin oxide based material. I am somewhat confused as to how this operates, as SnO will readily oxidize to SnO2, but SnO2 would tend to decompose at the operating temperature if power is not applied. The transition between the oxides would seem likely to ruin the structure the anode. I am not sure entirely how such an anode would be constructed, but it would possibly involve an indium oxide base layer as is used in some commercial electrodes. This could be electroplated with tin and then oxidized by anodizing. Another possibility is to electroplate tin oxide by anodizing in tin nitrate, similar to the method for making lead dioxide anodes. Either way, a base layer would likely be necessary to protect the base metal from oxidation by SnO2.

I am unsure on any alternatives.




The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
not_important
International Hazard
*****




Posts: 3873
Registered: 21-7-2006
Member Is Offline

Mood: No Mood

[*] posted on 3-11-2008 at 06:52


Hard to tell what they are using, and there's no experimental detail

These links may be of interest:

http://www.teco.com/products/Documents/TinElectrodes.pdf

http://www.dysontt.com/downloads/Tin%20Oxide%20Electrodes.pd...

http://www.wipo.int/pctdb/en/wo.jsp?IA=NO2007000049&wo=2...
View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 3-11-2008 at 13:01


Tin dioxide is the standard resistive heating element for doing precision glass melts; it's used much like silicon carbide, sintered into rod form with electric contacts brazed or pressed on at the ends. It's likely the "tin-oxide" of the document sited actually refers to SnO<sub>2</sub>.
View user's profile View All Posts By User
dann2
International Hazard
*****




Posts: 1523
Registered: 31-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 3-11-2008 at 15:37


Quote:
Originally posted by kilowatt
Another possibility is to electroplate tin oxide by anodizing in tin nitrate, similar to the method for making lead dioxide anodes.

Hello,
Just wondering how that is done. Tin Nitrate does not really exist as such.

Cheers,
DANN2
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 4-11-2008 at 01:20


I think it does in very concentrated nitric acid. It precipitates as SnO2 on contact with water. Probably not very practical though.

It might not be too difficult to make a sintered SnO2 electrode from fine clay-like powder. Its melting point is low for an oxide; most sources say 1127°C.

[Edited on 4-11-2008 by kilowatt]




The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
dann2
International Hazard
*****




Posts: 1523
Registered: 31-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 4-11-2008 at 01:43


Helllo,

There is a thread here may be of some use.
http://www.sciencemadness.org/talk/viewthread.php?tid=8253&a...

There is also a pile of SnO2 anode related stuff in the 'More on PbO2 anodes' thread.
SnO2 is usually made by heating Stannic Chloride. This if for thin film anodes (ie. coated on Ti or other substrate).

I though Tin Oxide was an extreme refractory.
Dann2
View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 4-11-2008 at 04:16


SnO<sub>2</sub> used as electrodes is typically doped with Sb or As to enhance its semiconducting properties. Sintering aids are CuO and/or ZnO. Not the easiest small-lab manufacturing project. Rather than build, buy. not_important posted a couple of links to manufacturers. My information is from <i>Electroceramics</i>, by Moulson and Herbert.
View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 4-11-2008 at 04:36


Frustratingly, I can't seem to find consistent information on the melting point of SnO<sub>2</sub>. The WebElements page lists one at 1630&deg;C. Certainly the Wikipedia entry of 1127&deg; C is probably wrong, given that this material is used at temperatures significantly above that. (That figure also appears in MSDS pages, which is where, I'm assuming, the Wikipedia value came from.)
View user's profile View All Posts By User
ycheff
Harmless
*




Posts: 5
Registered: 18-10-2008
Member Is Offline

Mood: No Mood

[*] posted on 4-11-2008 at 07:19


Chapman and Hall data base also gives 1630 for mp and 1800-1900 for bp.
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 4-11-2008 at 09:04


Quote:

Certainly the Wikipedia entry of 1127° C is probably wrong

At least 4 different MSDS's state 1127° C, but I have seen 1630°C a few times too. I just went with the one that was seen more.

About buying the anodes: in theory the undoubtedly high cost might not be such an issue for an already expensive and high productivity cell. What I don't like is the low surface area that all the commercial anodes seem to have, possibly not suitable for the high current (several kA) of even a mediocre sized FFC Cambridge cell. I wonder they are very porous, as this would increase the surface area.

The film deposition methods using SnCl4*5H2O and SbCl3 look like the most straightforward, but I am confused on one point about these. When heating the coating to high temperature to oxidize SnCl4 to SnO2, how is it that the majority of the SnCl4 does not boil away? It seems unlikely to me that it would remain well enough to form a coating on anything by carrying out the process in an open system.

[Edited on 4-11-2008 by kilowatt]




The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
dann2
International Hazard
*****




Posts: 1523
Registered: 31-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 4-11-2008 at 15:06


Hello,

Perhaps some of the Stannic Chloride goes off as vapour before it converts to Oxide but the procedure definitely works.
I have no idea if this type of anode is suitable for what you want to do.
The prodecure below if from a guy who made lots of anodes at college.
(leave out the bits regarding PbO2)
This is my procedure to prepare Ti/PbO2 anode with SnO2+SbOx(Sb2O5+Sb2O3) inter layer.
The Ti plates (5 × 1 × 0.1 cm) were used as substrates. Prior to using as substrates, they were polished with 320-grit sandpaper, degreased in 40 wt% NaOH solution at 80C for 2h, etched in a boiling 10 % oxalic acid solution during 1 h, after that, they were rinsed with distilled water and dried naturally. (If you don't have oxalic acid solution,sometime concentrated hydrochloric acid also works, you should see a purple solution during the boiling Ti plate, this step is very important, only via this you can remove the TiO2 insulting layer,Remember: do not use raw water in this step, a distilled water is preferred.
The SnO2+Sb interlayer was prepared following a standard thermal decomposition method and the procedures were as follows:
A solution containing SnCl4:5H2O and SbCl3 was dissolved in a mixture of n-butanol(or ethonal)+HCl.(eg. 4g SnCl4:5H2O + 0.2g SbCl3 + 9ml n-butanol + 1ml HCl solution, you can made about 5 anodes, the best mol ratio is SnO2: Sb=100:4~8). The precursor solution was distributed onto the pretreated Ti plates by brushing. The solvent was dried in air or a oven(90C,a hair dryer also ok), and the electrode was introduced into an oven at 450C for 10 min for the decomposition of the salt and the formation of the metal oxides. This process was repeated for 15-20 times. A final annealing of the electrode was performed at about 500C for 1h.

Anodes like this are sometimes used for wastewater treatment.


Dann2
View user's profile View All Posts By User
chief
International Hazard
*****




Posts: 630
Registered: 19-7-2007
Member Is Offline

Mood: No Mood

[*] posted on 4-11-2008 at 18:05


From Wikipedia, the Tin-solubilities:
Tin(II) bromide SnBr[2] 85
Tin(II) chloride SnCl[2] 84
Tin(II) fluoride SnF[2] 30
Tin(II) iodide SnI[2] 0.99 1.17 1.42 2.11 3.04 3.58 4.2
Tin(II) sulfate SnSO[4] 18.9

Maybe for SnO2-electrodepositing the sulfate might be used instead of the nitrate (really not existing ?),
==> since that would be an analogy to the PbO2-manufacturing within H2SO4; only that SnSO4 is water-soluble, while PbSO4 is not; thats why with PbO2 the nitrate has to be used ... ?

Also: Usually the SnO2-electrodes are sprayed, but this is because it is applied as one of the few transparent conducting materials, at solar-cell-surfaces etc. . Since the substrates are not conducting, the SnO2 must be applied another way (not anodizing).

But anyhow a good description of making SnO2-layers might be interesting, because I since a while like the idea of trying some solar-cells (CuO is said to work at 2 % efficiency,; with In one could reach 10 % by CuInS2; maybe other materials can be used too, need to be semiconducting (like many sulfides are))

[Edited on 4-11-2008 by chief]
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 5-11-2008 at 11:41


kilowatt, I want to know what spurred your interest in the FFC Cambridge Process.

I could only imagine that a SnO2 based electrode would not hold up in the molten chloride bath for a long protracted time of cell operation (perhaps a eutectic would be necessary to retard erosion at lower temperatures). I constructed a rudimentary cell based on the FFC Cambridge Process and I have to say that although graphite erodes, it definitely works and the cost of replacing graphite certainly doesn't exceed the energy, time and cost of making SnO2 electrodes that may or may not be "permanent" in the sense that they would never have to be replaced.

What are you hoping to produce from the process, just curious?




As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 5-11-2008 at 12:46


I had read about the FFC Cambridge process for titanium production, then a suggestion by not_important in the magnesium thread got me thinking about the potential it has for refining all manners of metals and semi-metals. I am looking to experiment with the feasibility of refining such various metals and semi-metals such as mentioned in my FFC capabilities thread with this type of calcothermic reduction cell, and put to use what I find.

What temperature did you run your cell at? Did you use a eutectic? The documentation I have seen indicates that graphite is consumed entirely, in other words practically no uncombined oxygen is produced when it is used as an anode material. Are you sure this wasn't the case with your cell too? The cost of replacing graphite in this case would be VERY prohibitive if we are talking about large runs. It was also indicated that the SnO2 anode showed very little erosion after a 12 hour run. After all, what would it be oxidized to?




The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 5-11-2008 at 16:25


Oh yes, the graphite was certainly eroded to hell to say the least. But I have been experimenting with small runs with boron reduction so it has not been too much of a problem for me. I suppose you are looking more towards a large scale production.

I did not use a eutectic and ran the cell at approximately 950 degrees Celsius. It would be very interesting to see if a SnO2 anode could be produced at the home-chemist level, and I am all for it especially now that you mention there was little erosion for 12 hour runs. Well, after looking over this thread, I am going to experiment with SnO2 electrodes to see what I can get out of it.




As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 5-11-2008 at 18:53


I'm curious, how did the boron extraction go? This is one of the things I want to try with my cell. Also how did you apply it to the cathode? Did you just dip it in fused boric oxide? I wonder if adding soda or another additive to the boric oxide would allow the use of granules or powder (thus much more porous and effective than a fused mass) with a melting point above the cell operating temperature. Sodium should be distilled out while the boron remains at the cathode.

[Edited on 5-11-2008 by kilowatt]




The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 5-11-2008 at 19:17


Not very well. There was a ton of carbon debris and the cell body (a titanium container, I think it was alloyed with something that corroded it far too much to be pure titanium) added a lot of oxidized junk into the chloride melt, so it was hard to determine whether I had boron or not. I'm working on modifying the cell sometime this weekend and giving it another run.

I thought about using sodium borate, but I couldn't figure out a way to contain the sodium if it distilled off and it would have been a severe hazard to myself as my cell isn't particular well constructed in general. I just added the powdered boric acid first, heated the cell until the boric acid dehydrated/melted to boron oxide, then added the calcium chloride and heated it to the stated temperature. I wish I had some welding gear so I could construct the cell with some steel but at the time being I neither have the means nor the finances to undertake a total reconstruction of the cell. Meh, you do what you can with what you have right?




As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 5-11-2008 at 19:23


What was your cathode and how did you keep the oxide on it? I planned to use changeable cathodes with maybe a fine steel screen, but have a separate cathodic protection supply connected to the container which would run at low power and should eliminate corrosion. The close proximity of the cathodes to the outer wall may be enough for cathodic protection. Doubling the container as the cathode would be ideal but that would not be a very versatile or efficient setup in my opinion.



The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 5-11-2008 at 19:30


Ha ha, funny that you say that, because I used my container as the cathode. It seemed easier at the time, but that was my faulty assumption; I'm just lucky the chloride melt didn't get into the heating elements or the refractory. From my understanding of the process, the oxide-to-be-reduced doesn't need to be in contact with the cathode per se, it simply needs to be in contact with the dissolved calcium in the chloride melt. But maybe that's why my container corroded to hell. I'll try using a separate cathode in this next run just to see if anything actually happens.



As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 5-11-2008 at 19:36


Yes, it is true that the oxide does not need to be in electrical contact with the cathode (it's often an insulator anyway), but I believe it helps if it is in close proximity, because it is more calcium-rich near the cathode. The cathode (and thus container if you used it as such) should be protected from oxidation or dissolution in the electrolyte by the calcium metal that is formed at its surface. At least this would be the case if your container/cathode was not very miscible with calcium, such as I understand is the case with steel. Perhaps this is not necessarily the case with titanium? What sort of voltage/current and current density did you get? My understanding is the experimental FFC Cambridge cells run about 2-3V (preferably controlled during the process so it is decreased as the run progresses) and about 1A/cm^2.



The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 6-11-2008 at 17:08


I was working with about 5 volts and low current density (100 mA/cm^2), basically all that I had around. I wasn't sure (and am still not) where I can get a dedicated power supply with controllable low voltage and high current.

What kind of power supply are you hoping to use and what material are you using for the cathode? SnO2?




As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
tentacles
Hazard to Others
***




Posts: 191
Registered: 11-11-2007
Member Is Offline

Mood: No Mood

[*] posted on 6-11-2008 at 18:42


bereal: Look on eBay for power supplies.. A good set of search terms is "kepco" "lambda EMS". I picked up a 5v/200A CC/CV supply (no gauges though, but that's easy to fix) for $50 shipped. And it's efficiency rating is over 75%. Be sure to search under power supplies.. I suggest doing the lambda search from the start page, and then going to the category from there. Otherwise it's a PITA trying to figure out ebay's categories.

What part of manitoba are you in? I'm in Winnipeg.
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 7-11-2008 at 11:04


Thank you so very much tentacles, I've been looking around for something like this for a while. I'm actually in Manhattan Beach, California, I think I'll change that for unambiguity :).



As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
kilowatt
National Hazard
****




Posts: 322
Registered: 11-10-2007
Location: Montana
Member Is Offline

Mood: nitric

[*] posted on 7-11-2008 at 13:15


I intend to use a large set of automotive alternators (these can be had quite cheaply) for my large cell in the future, and a 100A battery charger I have for small experimental cells. There would be a set of alternators for each individual cathode, so that each cathode's voltage can be controlled independently via the alternators' exciter current. I am considering running the alternators off a heat engine such as a Stoddard engine (which can be made from a pair of modified 4 cycle engines) which operates from heat exchangers on the cell's inner wall, so that the entire apparatus runs on gas burners or another heat source. The maximum Carnot efficiency of such a setup would be about 75%, but quite a bit lower in reality. This way much of the waste heat that results from the cell's low current efficiency would be used to power the cell's electrical supply, which would operate entirely on fuel or any heat source. If properly located, the heat exchangers should encourage convection currents within the electrolyte too, possibly increasing cell performance.

SnO2 cathodes? The entire point of an FFC Cambridge cell is to reduce oxides to metal.:P I plan to use steel or inconel cathodes and an SnO2 coated welded steel or cast monel anode.




The mind cannot decide the truth; it can only find the truth.
View user's profile View All Posts By User
bereal511
Hazard to Others
***




Posts: 162
Registered: 9-8-2005
Location: Madison, WI
Member Is Offline

Mood: No Mood

[*] posted on 8-11-2008 at 17:40


Hahaha, I mean anode* for SnO2.



As an adolescent I aspired to lasting fame, I craved factual certainty, and I thirsted for a meaningful vision of human life -- so I became a scientist. This is like becoming an archbishop so you can meet girls.
-- Matt Cartmill
View user's profile View All Posts By User
 Pages:  1  

  Go To Top