Dissolution of Copper and Steel by Molten Aluminum
Is anyone able to get access to this paper from the National Academy of Forensic Engineers?
Journal Article Title: Dissolution of Copper and Steel by Molten Aluminum
Article Author(s): FUCHS, RODNEY G., P.E.
Volume: 14
Volume #: 2
Month: December
Year: 1997
Download this paper
Abstract:
Fire investigators occasionally find metals such as steel and copper melted, pitted, and eaten away in a fire scene where temperatures have obviously
not reached the melting point of these metals. Molten metal, such as aluminum, can actually dissolve steel and copper at temperatures below their
normal melting points. This paper discusses the phenomenon along with the ramifications to the investigator of the origin and cause of a fire.
Thanks
|
|
|
vyper47
Harmless
Posts: 12
Registered: 16-4-2020
Member Is Offline
|
|
Couldn't download the exact paper you requested, but found something related, that might come to help
https://sci-hub.tw/10.2320/matertrans1960.23.780
|
|
|
Irish9
Harmless
Posts: 3
Registered: 28-12-2015
Location: Victoria Australia
Member Is Offline
Mood: No Mood
|
|
I don't have access to the papers but I have observed that personally. I make my own steel crucibles for casting a range of metals and was tinkering
with greensand casting of Aluminium and had a crucible fail. It was eaten though at the base (hottest part with this furnace) from the inside out.
Would have been a lot more interesting if it had not dropped two kg of Al alloy into the bottom of a newish furnace
|
|
|
j_sum1
Administrator
      
Posts: 5760
Registered: 4-10-2014
Location: Unmoved
Member Is Offline
Mood: Possessor of a tidy and organised lab. Now to mess it up again.
|
|
It is small, but that 5°C drop down to the eutectic at 98%Al is enough to do it.
https://www.researchgate.net/profile/Qingyou_Han/publication...
And it is amazing how often the minute details of phase diagrams is where all the critical action is.
|
|
|