RU_KLO
Hazard to Others
 
Posts: 321
Registered: 12-10-2022
Location: Argentina
Member Is Offline
|
|
Crucible for NaOH fusion
I need to perform fusion with NaOH + NaNO3 + Na2CO3.
the book asks for nickel crucible.
I read the wiki crucible:
https://www.sciencemadness.org/smwiki/index.php/Crucible
Getting a Nickel or magnesium oxide is difficult for me.
In another posts:
"The one time I melted NaOH in a porcelain crucible, I ended up destroying it by simply dissolving/weakening the ceramic to the point of failure. I've
never had this problem with metal crucibles "
http://www.sciencemadness.org/talk/viewthread.php?tid=154253...
"But as mackolol said plain ceramic should be ok, I also did a lot with molten NaOH and KOH in them"
https://www.sciencemadness.org/whisper/viewthread.php?tid=15...
the procedure ask for a NaOH "bed" in the bottom of the crucible, the sample (fine ground) above this bed and in the middle, on top a layer of NaNO3 +
Na2CO3.
heat (slowly) till everything dissolves. (no more that 15 sec in a nickel crucible)
Can this be "substituted" with a common porcelain crucible (which I can get)
I understand that alkaly (molten even more) attacks porcelain, but maybe not too hot (only until melting) and 10s there is no such attack or is minor.
(more important, not contaminating the sample - or trace contamination that will not invalidate the analysys)
Does anyone has experience with this?
Thanks
Go SAFE, because stupidity and bad Luck exist.
|
|
|
Rainwater
National Hazard
  
Posts: 993
Registered: 22-12-2021
Member Is Offline
Mood: Break'n glass & kick'n a's
|
|
So any type of ceramic material (ether Al or Si based) will dissolve is this mixture.
So will aluminum containers
You need nickel or platinum to prevent contamination of your product.
Cheap stainless, cast iron, etc will intorduce iron contamination turning your molten salt a black, then brown, then red
Good stainless will introduce crome turning first a light blue then a darker blue.
If this will effect your chemistry is unknown to me
I use these little cups with molten NaOH.
https://www.amazon.com/gp/aw/d/B06XZB1ZG2
[Edited on 10-1-2025 by Rainwater]
"You can't do that" - challenge accepted
|
|
|
metalresearcher
National Hazard
  
Posts: 822
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
Amazon does sell Ni crucibles.
https://www.amazon.com/s?k=nickel+crucible&crid=2HCLRQQR...
Ni is rather restistant to molten lye. NaOH with the other two salts dissolved in it is still very aggressive to most other materials.
Pt is the best but very $$$.
|
|
|
RU_KLO
Hazard to Others
 
Posts: 321
Registered: 12-10-2022
Location: Argentina
Member Is Offline
|
|
Understand, thanks.
Could one made of graphite work? Or graphite will be corroded too?
I don't mind carbon contamination.
Go SAFE, because stupidity and bad Luck exist.
|
|
|
metalresearcher
National Hazard
  
Posts: 822
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
Quote: Originally posted by RU_KLO  | Understand, thanks.
Could one made of graphite work? Or graphite will be corroded too?
I don't mind carbon contamination. |
Graphite will be corroded I think, but it is an assumption. I have never tried.
|
|
|
unionised
International Hazard
   
Posts: 5142
Registered: 1-11-2003
Location: UK
Member Is Offline
Mood: No Mood
|
|
Silver works if you aren't getting too hot.
|
|
|
yobbo II
National Hazard
  
Posts: 823
Registered: 28-3-2016
Member Is Offline
Mood: No Mood
|
|
Can you use a 'skull' of the mixture?
Use large dish to hold the stuff and heat from the top.
The container does not see much heat
|
|
|
DraconicAcid
International Hazard
   
Posts: 4519
Registered: 1-2-2013
Location: The tiniest college campus ever....
Member Is Offline
Mood: Semi-victorious.
|
|
I got nickel crucibles off of AliExpress that worked fine for me.
Please remember: "Filtrate" is not a verb.
Write up your lab reports the way your instructor wants them, not the way your ex-instructor wants them.
|
|
|
walruslover69
Hazard to Others
 
Posts: 243
Registered: 21-12-2017
Member Is Offline
Mood: No Mood
|
|
I have used both a graphite crucible and a stainless steel cocktail tumbler to heat NaOH + cyanuric acid+ sodium carbonate up to 800C for cyanide
synthesis and it worked well. Both crucibles looked worse afterwards. You could maybe run the reaction twice before the crucibles failed, but they
didn't seem to significantly contaminate the reaction. A bunch of black graphite dust carried through, but nothing that a quick filtration through a
sand column can't fix!
depending on your budget a nickel crucible would be really nice to have.......
|
|
|
Sulaiman
International Hazard
   
Posts: 3953
Registered: 8-2-2015
Member Is Offline
|
|
Although not expensive in general
chemistry equipment terms,
they are not in my 'disposable' price range
(equiv.USD13or18 for 30or50ml with lid)
So, how re-usable are nickel crucibles
when used for reactions that require a nickel crucible?
CAUTION : Hobby Chemist, not Professional or even Amateur
|
|
|
Keras
International Hazard
   
Posts: 1149
Registered: 20-8-2018
Location: (48, 2)
Member Is Offline
|
|
I have a nickel (or is it stainless steel? I think it’s nickel) crucible, and there’s no problem reusing it over and over. I used it for several
high temperature fusions, such as making p-cresol from sodium p-toluenesulphonate or recently indigo from phenylglycine o-carboxylic acid.
What I usually do is scrape it with a rag full of some cleaning/polishing paste, such as 'The Pink Stuff™'.
|
|
|
Fleaker
International Hazard
   
Posts: 1254
Registered: 19-6-2005
Member Is Offline
Mood: nucleophilic
|
|
I used to use graphite for molten KOH all the time. It does get corroded, but I was doing kilo scale fusions in an induction heater with a graphite
crucible.
I will say this much--contrary to what is reported--platinum is not a good material for fusions that see air. Any air and there is a problem.
Excusing gold, I think zirconium is best, followed by nickel, then nickel alloys like the inconels. Then plain iron.
I have done many a NaOH/NaNO3 in iron, at rather large scale where the iron products didn't matter. Safer at below 400 C. Higher than that, and Ni or
Zr.
Neither flask nor beaker.
"Kid, you don't even know just what you don't know. "
--The Dark Lord Sauron
|
|
|