Author: Subject: Calcium Oxide from sea shells
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 17-9-2014 at 07:05
Calcium Oxide from sea shells


Hi,
I have been reading and came across a reference to calcium oxide in times gone by, being made from crushed sea shell's. As I live 4 miles from a deserted fabulous beach full of sea shells, this has me thinking.
Apparently the shells are crushed and heated to above 850C, the time of heating wasnt given however. We have a very small granite stone kiln we built outside last year, it has been used for melting lead for fishing weights and some Aluminum. The fuel source was dried pine cones (what else :D) that burn very hot and are fairly dense in a way similar to hard wood, they are also a renewable source.
The kiln is fanned from several small high powered 12V fans run from a leisure battery. I am confident I can reach and maintain the temperature but I am not sure for how long this needs to be done.
While I would wash the shells well in tap water, I am pretty sure any organic material would simply burn off or at most be converted to carbon. Calcium oxide looks like a neat desiccant and while not overly expensive 500 grams on ebay with postage is around £7.
So any idea how long the >850c needs to be held for? I might make a 2 KG batch and store in several smallish containers. I also need another crucible as the last one got broken.
View user's profile View All Posts By User
DJF90
International Hazard
*****




Posts: 2266
Registered: 15-12-2007
Location: At the bench
Member Is Offline

Mood: No Mood

[*] posted on 17-9-2014 at 08:49


Plante1999 has done this exact preparation and reported his results in the Prepublications forum.
View user's profile View All Posts By User
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 17-9-2014 at 08:54


Quote: Originally posted by DJF90  
Plante1999 has done this exact preparation and reported his results in the Prepublications forum.


Ok thank you I will go have a look :D
View user's profile View All Posts By User
Magpie
lab constructor
*****




Posts: 5939
Registered: 1-11-2003
Location: USA
Member Is Offline

Mood: Chemistry: the subtle science.

[*] posted on 17-9-2014 at 09:13


Plante specifies 800°C for one hour. I have made CaO from garden lime [very cheap source of slaked lime, Ca(OH)2] a number of times. IIRC I used conditions very similar to that of Plante.

This makes a nice experiment for the use of a little chemistry math. Weigh your lime before and after heating. Then see if the weight loss matches the theoretical loss obtained by calculation using molecular weights.




The single most important condition for a successful synthesis is good mixing - Nicodem
View user's profile View All Posts By User
metalresearcher
International Hazard
*****




Posts: 693
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 17-9-2014 at 10:09


Quote: Originally posted by Magpie  
Plante specifies 800°C for one hour. I have made CaO from garden lime [very cheap source of slaked lime, Ca(OH)2] a number of times.


Indeed that worked for me too. Just a bag of garden (?) lime from the hardware shop. I heated 500g in a Kanthal furnace for an hour to 700C and I saw some plumes of water escape.

I used it for arcing it with bbq charcoal to make CaC2 whcih succeeded.
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 17-9-2014 at 10:41


Quote: Originally posted by metalresearcher  
I used it for arcing it with bbq charcoal to make CaC2 whcih succeeded.

Wow !

What arc did you use ?
A stick welding rig ?




View user's profile View All Posts By User
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 17-9-2014 at 12:04


Quote: Originally posted by Magpie  
Plante specifies 800°C for one hour. I have made CaO from garden lime [very cheap source of slaked lime, Ca(OH)2] a number of times. IIRC I used conditions very similar to that of Plante.

This makes a nice experiment for the use of a little chemistry math. Weigh your lime before and after heating. Then see if the weight loss matches the theoretical loss obtained by calculation using molecular weights.

Some of the shells like mussel and razor clam will have organic material, I could burn that off with a bunsen I guess.
But yes it will be interesting to see the results. A couple of questions that have arisen from a cryptic conversation with my dad........

I am assuming that shells are calcium carbonate, I mentioned this to dad and he smiled and asked if I was sure??? Looking at a shell under the microscope I think I am wrong. So working on an assumption I think there s some magnesium carbonate in there as well, there is definitely something other than calcium carbonate because I can see two crystal like structures that are different (mag Oil Immersion 1400x with phase contrast no stain).
So if I assume mag carbonate my question is there a test to distinguish magnesium and calcium carbonate?
Its not that I think it will matter, but I would like to know. Not sure what our home built stone kiln/roket stove can do temperature wise,but we have a IR thermometer that goes upto 1200C and it easily passes that! its pretty efficient on dry large pine cones, I burnt around 30Kg of cones last year melting a load of aluminum cans! Actually I ended up with 31Kg of aluminum! Mostly cans I picked up on our road verge and the lay by near us, also the beach had loads and the can recycle bank is full most days, so people just put bags of cans by the side. I pick them up and store until dad gets fed up falling over cans lol.
Anyway weighed the aluminum in and it paid for a new function generator :D.
All the ash that was left came to under 500g! The inside of the kiln is lined with lime and fire fibre mix (no idea what it is made of). I want to build a slightly bigger one this winter.
View user's profile View All Posts By User
careysub
International Hazard
*****




Posts: 1339
Registered: 4-8-2014
Location: Coastal Sage Scrub Biome
Member Is Offline

Mood: Lowest quantum state

[*] posted on 17-9-2014 at 19:05


Quote: Originally posted by Little_Ghost_again  
Quote: Originally posted by Magpie  
Plante specifies 800°C for one hour. I have made CaO from garden lime [very cheap source of slaked lime, Ca(OH)2] a number of times. IIRC I used conditions very similar to that of Plante.

This makes a nice experiment for the use of a little chemistry math. Weigh your lime before and after heating. Then see if the weight loss matches the theoretical loss obtained by calculation using molecular weights.

Some of the shells like mussel and razor clam will have organic material, I could burn that off with a bunsen I guess.
But yes it will be interesting to see the results. A couple of questions that have arisen from a cryptic conversation with my dad........

I am assuming that shells are calcium carbonate, I mentioned this to dad and he smiled and asked if I was sure??? Looking at a shell under the microscope I think I am wrong. ...


Biological structural materials usually have nanostructure patterning that make them look different from minerals with similar composition - part of the evolutionary engineering that gives them superior physical properties .

If you are going to calcine them all of the organic materials (like chitins, proteins, etc) that may be incorporated into the structure are going to disappear.

Looking at one source that looked at the mineral composition of calcined mussel and oyster shells:
http://www.scielo.br/scielo.php?script=sci_arttext&pid=S...
we see that mussel shells are 95.6% CaO, with roughly similar amounts of seven other minerals (0.4 to 0.9%), while oyster shells are almost pure CaO - 98.2%.
View user's profile View All Posts By User
Zyklon-A
International Hazard
*****




Posts: 1547
Registered: 26-11-2013
Member Is Offline

Mood: Fluorine radical

[*] posted on 18-9-2014 at 06:20


Quote: Originally posted by aga  
Quote: Originally posted by metalresearcher  
I used it for arcing it with bbq charcoal to make CaC2 whcih succeeded.

Wow !

What arc did you use ?
A stick welding rig ?

You can read about it here:http://www.sciencemadness.org/talk/viewthread.php?tid=27475#...




View user's profile View All Posts By User
Bert
Super Administrator
*********




Posts: 2747
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 18-9-2014 at 06:48


If you are intending to re-create traditional building materials?

http://homescale.wordpress.com/makinglime/

Be sure to wash all the sea salt off the shells, especially if you're going to use steel mesh or bars in concrete work.




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
blogfast25
Thought-provoking Teacher
*****




Posts: 10340
Registered: 3-2-2008
Location: Old Blighty
Member Is Offline

Mood: No Mood

[*] posted on 18-9-2014 at 10:09


Have a look at this for a better understanding of the relation between temperature and CO2 partial pressure, when calcining CaCO3 to lime and CO2:

http://en.wikipedia.org/wiki/Calcium_carbonate#Calcination_e...




View user's profile Visit user's homepage View All Posts By User
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 18-9-2014 at 10:15


Thanks guys for the links.
I dont want it to build with, I just thought it would be handy to have and a fun thing to do. It also gives me an excuse to fire up the kiln :D
View user's profile View All Posts By User
Actinium
Hazard to Self
**




Posts: 67
Registered: 2-9-2014
Member Is Offline

Mood: synthetic

[*] posted on 18-9-2014 at 20:33


How fast does Ca(O) turn back into Ca(OH)2 ?
Doesn't it re-hydrate quite fast?
View user's profile View All Posts By User
blogfast25
Thought-provoking Teacher
*****




Posts: 10340
Registered: 3-2-2008
Location: Old Blighty
Member Is Offline

Mood: No Mood

[*] posted on 19-9-2014 at 04:05


Quote: Originally posted by Actinium  
How fast does Ca(O) turn back into Ca(OH)2 ?
Doesn't it re-hydrate quite fast?


Not if stored properly.

But the reaction between fresh quicklime (CaO) and actual water can be quite vicious and needs to be done carefully. It was in Roman times one of the less enjoyable jobs to turn quicklime into slaked lime, allegedly...




View user's profile Visit user's homepage View All Posts By User
Bert
Super Administrator
*********




Posts: 2747
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 19-9-2014 at 04:55



Quote:

the reaction between fresh quicklime (CaO) and actual water can be quite vicious


A Mason jar full of quick lime with a few small holes punched in the lid has been used for fishing by resourceful hillbillies without access to dynamite... Throw it in the water, it sinks to the bottom and water enters. As the lime slakes, it heats, water boils and the holes clog from bits of lime being forced against them from inside. The eventual steam explosion of the jar may be sufficient to stun fish.




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
macckone
International Hazard
*****




Posts: 2140
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 19-9-2014 at 06:32


Quote: Originally posted by Bert  

Quote:

the reaction between fresh quicklime (CaO) and actual water can be quite vicious


A Mason jar full of quick lime with a few small holes punched in the lid has been used for fishing by resourceful hillbillies without access to dynamite... Throw it in the water, it sinks to the bottom and water enters. As the lime slakes, it heats, water boils and the holes clog from bits of lime being forced against them from inside. The eventual steam explosion of the jar may be sufficient to stun fish.

Have you been spying on my fishing?
View user's profile View All Posts By User
Actinium
Hazard to Self
**




Posts: 67
Registered: 2-9-2014
Member Is Offline

Mood: synthetic

[*] posted on 19-9-2014 at 13:14


Quote: Originally posted by Bert  

Quote:

the reaction between fresh quicklime (CaO) and actual water can be quite vicious


A Mason jar full of quick lime with a few small holes punched in the lid has been used for fishing by resourceful hillbillies without access to dynamite... Throw it in the water, it sinks to the bottom and water enters. As the lime slakes, it heats, water boils and the holes clog from bits of lime being forced against them from inside. The eventual steam explosion of the jar may be sufficient to stun fish.

My friend from W. Va will love this one:P
See Chemistry has very practical applications.

Now as far as drying the Ca(OH)2 > Ca(O) since I no longer have my kiln, will a torch suffice? If so I would use the bottom of a wine bottle so as not to ruin my precious glassware for this.
View user's profile View All Posts By User
blogfast25
Thought-provoking Teacher
*****




Posts: 10340
Registered: 3-2-2008
Location: Old Blighty
Member Is Offline

Mood: No Mood

[*] posted on 19-9-2014 at 14:08


Quote: Originally posted by Actinium  
Now as far as drying the Ca(OH)2 > Ca(O) since I no longer have my kiln, will a torch suffice? If so I would use the bottom of a wine bottle so as not to ruin my precious glassware for this.


It'll be borderline as the dehydration of slaked lime only starts at about 512 C.




View user's profile Visit user's homepage View All Posts By User
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 20-9-2014 at 03:36


Maybe you could use the fire bricks (slates) from inside something like a old broken wood burning stove.
Our MK2 kiln will use these to line inside the stone, we have no way to measure such high temps but I know the MK1 got extremely hot as the 1/2 inch steel sheet that the crucible was stood on melted!
The new Mk2 now under construction is going to use a fan from a kids small bouncy castle.
The air out put is very impressive, for control I am going to add a variac, this way I can control the amount of air going into the kiln.
Sone of the conifer trees in our wood produce huge 10" long pine cones (I use inches on here because most of you do, I prefer metric so if I get the sizes wrong sorry). When these cones are dry the are extremely dense, they make idea fuel for rocket stoves and kilns like this.
Our kiln designs have a burning chamber that is just behind the main flue, we place the object to be heated 6 inches up inside the flue. Just behind the fire chamber is the fuel box, this is where we put the cones, we can then poke them into the fire chamber and close the stone lid on the fire box.
What we found was as long as the flue (chimney) was 3 x the height as the fire box is long, then you get a massive updraft through the flue, this really gives a good draw on the fire. Add in extra air via a fan or whatever and you can get really high temperatures, most the rock around here is granite with marble here and there, we also have a area with lime stone but for the kiln we use the granite.
Everything is then rendered with cement and the fire fibre mix, then the fire bricks/tiles from wood burners go in front of this.
Hope that helps someone.
View user's profile View All Posts By User
Refinery
National Hazard
****




Posts: 371
Registered: 17-2-2014
Member Is Offline

Mood: Still

[*] posted on 20-9-2014 at 14:05


Calcium hydroxide decomposes to oxide at 550-600C, while calcium carbonate needs 850-900C, but practically it is necessary to take the temp over 950-1000C to make the reaction fast. I have made CaO with electric furnace from calcium carbonate, and when temperature reached 1000C, the mass was fully decomposed to the extent I could measure it.

I made a furnace on a small 60 liter steel drum. I cut it about 1/3, put some pearlite clay on bottom of it, placed two firebricks on top of them, sat a plastic bucket in the middle and poured calcium sulfate plaster. When it dried, I made holes for nichrome wire and casted the 1/3 drum head full of plaster with couple of reinforcing bars that act as a handle too, mantled the whole setup in 150mm thick rockwool slab and dumped it into a 208l drum. It has to be heated very carefully at first time and ideally it should be placed into oven at 60C for 4-6 hours and then for 100C for another 4 hours, and then slowly heated to operational temperature to drive out the moisture contained in the plaster. It may still crack, but the drum keeps it together and once it's cracked, thermal expansion wont hurt it anymore. It can withstand 1300c temps continously.
View user's profile View All Posts By User
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 22-9-2014 at 08:43


Electric is expensive here, mostly we run from a diesel generator. Also I like the idea of running from a renewable fuel. We have a 8 acre commercial plantation of spruces etc as part of our woodland. Pine cones litter floor everywhere here! Dried out the are very dense and burn like a really good hardwood.
Add a good blast of air and 1000C is not hard to achieve. I like the idea of your electric one and if electric was cheap here I would tempted because I could combine it with my love of electronics to make a control system! But its just easier and cheaper for us to use a granite wood fired kiln.
View user's profile View All Posts By User
blogfast25
Thought-provoking Teacher
*****




Posts: 10340
Registered: 3-2-2008
Location: Old Blighty
Member Is Offline

Mood: No Mood

[*] posted on 22-9-2014 at 11:35


Quote: Originally posted by Little_Ghost_again  
Add a good blast of air and 1000C is not hard to achieve. I like the idea of your electric one and if electric was cheap here I would tempted because I could combine it with my love of electronics to make a control system! But its just easier and cheaper for us to use a granite wood fired kiln.


Fairly easy: lots of fuel and lots and lots of air. It'll melt copper quite easily if you push it.

But bear in mind that a wood or coal based fire will be quite rich in CO<sub>2</sub>, as one of the sources above indicated. This tends to push the equilibrium CaCO<sub>3</sub>(s) < === > CaO(s) + CO<sub>2</sub>(g) to left again (while temperature ushes it to the right).




View user's profile Visit user's homepage View All Posts By User
Bert
Super Administrator
*********




Posts: 2747
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 22-9-2014 at 12:15


Pine cones should make for a quite luminous fire- Perhaps you should explore harnessing that?

Reverberatory furnace

Traditional lime burning

[Edited on 22-9-2014 by Bert]




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
Little_Ghost_again
International Hazard
*****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 22-9-2014 at 12:19


Quote: Originally posted by blogfast25  
Quote: Originally posted by Little_Ghost_again  
Add a good blast of air and 1000C is not hard to achieve. I like the idea of your electric one and if electric was cheap here I would tempted because I could combine it with my love of electronics to make a control system! But its just easier and cheaper for us to use a granite wood fired kiln.


Fairly easy: lots of fuel and lots and lots of air. It'll melt copper quite easily if you push it.

But bear in mind that a wood or coal based fire will be quite rich in CO<sub>2</sub>, as one of the sources above indicated. This tends to push the equilibrium CaCO<sub>3</sub>(s) < === > CaO(s) + CO<sub>2</sub>(g) to left again (while temperature ushes it to the right).


Now thats interesting! Does using charcoal lower the CO2? Although I am not too sure how easy it is to turn cones into charcoal!
Probably the best approach is to go for maximum heat. The other thing is the shells will be in a crucible rather than amongst the fuel, I doubt that is going to make any difference with CO2 though.
View user's profile View All Posts By User
vmelkon
International Hazard
*****




Posts: 669
Registered: 25-11-2011
Location: Canada
Member Is Offline

Mood: autoerotic asphyxiation

[*] posted on 25-9-2014 at 07:22


Quote: Originally posted by Little_Ghost_again  
Quote: Originally posted by blogfast25  

Fairly easy: lots of fuel and lots and lots of air. It'll melt copper quite easily if you push it.

But bear in mind that a wood or coal based fire will be quite rich in CO<sub>2</sub>, as one of the sources above indicated. This tends to push the equilibrium CaCO<sub>3</sub>(s) < === > CaO(s) + CO<sub>2</sub>(g) to left again (while temperature ushes it to the right).


Now thats interesting! Does using charcoal lower the CO2? Although I am not too sure how easy it is to turn cones into charcoal!
Probably the best approach is to go for maximum heat. The other thing is the shells will be in a crucible rather than amongst the fuel, I doubt that is going to make any difference with CO2 though.


Charcoal has a lot of carbon of course and as you burn it, it produces CO2. I imagine the ratio CO2 to H2O is higher for charcoal compared to wood which has moisture and carbohydrates and cellulose.




Signature ==== Is this my youtube page? https://www.youtube.com/watch?v=tA5PYtul5aU
We must attach the electrodes of knowledge to the nipples of ignorance and give a few good jolts.
Yes my evolutionary friends. We are all homos here.