Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: CuSO4 electrolisis
Treason
Harmless
*




Posts: 5
Registered: 22-10-2006
Location: Colombia
Member Is Offline

Mood: Learning

shocked.gif posted on 22-10-2006 at 10:52
CuSO4 electrolisis


Could someone help me?

I'm studying chemistry but something anoying just happened when I was depositing Cu by the electrolisis of CuSO4. I used a Graphite electrode and made twice the experience. The first time I obtained 0.03g above what I should, so I made it once again, (with the teacher next to me) and obtained 0.023g below what I should.

Is there a reason for that? I dried the graphite after depositing the Cu so I don't know where could I be wrong.
View user's profile View All Posts By User This user has MSN Messenger
woelen
Super Administrator
*********




Posts: 7768
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 22-10-2006 at 11:04


The experimental conditions must be very precisely determined in order to check the charge/mass ratio. You should precisely measure the current as function over time (integral of current over time equals the total charge). Also, you should be sure, that there is no side reaction, in which hydrogen is formed. You even may have some hydrogen, absorbed into the metal, making it weigh less than you would expect. This kind of experiments is very hard to perform precisely. Best would be to have a current logging (e.g. every few seconds, you measure the average current over the past unit of time) and use the integrated value for computing the expected amount of plated copper.



The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
Waffles
Hazard to Others
***




Posts: 196
Registered: 1-10-2006
Member Is Offline

Mood: No Mood

[*] posted on 22-10-2006 at 11:33


Stone knives and bear skins. Experimental error. Human error. This should be moved to Beginnings.



\"…\'tis man\'s perdition to be safe, when for the truth he ought to die.\"
View user's profile View All Posts By User
The_Davster
A pnictogen
*******




Posts: 2861
Registered: 18-11-2003
Member Is Offline

Mood: .

[*] posted on 22-10-2006 at 11:45


You have to go into more detail about the equipment used, electrolysis experiments can be either very simple and not quantitative, or really complex with colombmeters and such. Without all the fancy equipment, I would not be expecting exact yields. Unfortunatly, electrolysis has all sorts of physics behind it which make it a bit more difficult than two electrodes in a solution. Without all the stuff Woelen mentioned, I would not expect yields precise to within 0.01g, which it seems you are expecting.



View user's profile View All Posts By User
Treason
Harmless
*




Posts: 5
Registered: 22-10-2006
Location: Colombia
Member Is Offline

Mood: Learning

[*] posted on 22-10-2006 at 12:00


I never tought that hydrogen could do things like that. I'll have to review all what we done once again and search where the error can be (Even when it can be everywhere or in more than in one place at the same time).
Thank you a lot. I'll keep reading.
View user's profile View All Posts By User This user has MSN Messenger
Magpie
lab constructor
*****




Posts: 5939
Registered: 1-11-2003
Location: USA
Member Is Offline

Mood: Chemistry: the subtle science.

[*] posted on 22-10-2006 at 20:01


How much did you expect to get?



The single most important condition for a successful synthesis is good mixing - Nicodem
View user's profile View All Posts By User
Ozone
International Hazard
*****




Posts: 1269
Registered: 28-7-2005
Location: Good Olde USA
Member Is Offline

Mood: Integrated

[*] posted on 23-10-2006 at 19:41


Hello,

Radio Shack was selling a very cool multimeter (self scaling, too) which compared well with my Fluke, AND, has a serial output. It comes with a very intuitive software package called "Meter View"tm which seems to work on win 95, 98, 2000, and XP (have not tried XP-64 or Vista beta). It gives you a nice graph, and outputs to ASCII wich is simple to import into Excel as a CSV. It cost me about $70 US imagine that, a Radio Shack product that is worth every penny.

You should use this to measure the current and cell voltage. The cell voltage can be used (look up the Nernst equation, viz. not-so-fun-damentals) to determine if the redox you are trying to do is even possible, and if it is, the current can be used to calculated the amount of metal deposited per unit of time.

Good luck, keep trying,

O3




-Anyone who never made a mistake never tried anything new.
--Albert Einstein
View user's profile View All Posts By User
Quibbler
Hazard to Self
**




Posts: 65
Registered: 15-7-2005
Location: Trinidad and Tobago
Member Is Offline

Mood: Deflagrated

[*] posted on 24-10-2006 at 05:49


Copper sulphate electrolysis should work, but you need to be careful.
A small current for a long time is what is required.
A large current and the CuSO4 concentration around the electrodes will diminish and other reactions will take place.

The conditions I use are 6 g of CuSO4.5H2O in 100 g H20 and a current of 10 mA regulated (with a LM317) for 2 hours.

Even so the cathode reaction is often not as pure as I would like.
If you can degassing the solution also helps.
View user's profile View All Posts By User

  Go To Top