[*] posted on 12-5-2017 at 23:29
Seperating chrome from iron and nickel, stainless steel


been curious about dragging chrome out of stainless steel because its quite abundant and the element chrome for whatever reason seems interesting to me, fancy colours or whatever

anyhow the common procedure for me is to dissolve it in HCl, thereafter NaHCO3 it into basic chromium hydroxide, filter that off (along with lots of iron and nickel hydroxide)
react that with NaClO, then NaCrO4 is produced, it can at this point then be fractionally recrystallized, possibly crystallizing it as large crystals hoping it wont co-crystallize with other nasties in solution

anyhow.. it seems that chromium oxalate is quite soluble, more than 100g/100mL, i dont get why it would be, it seems like it doesnt quite follow the system metal oxalates usually do, where nickel and iron are quite insoluble

Nickel oxalate NiC2O4.2H2O 0.00118
Iron oxalate dihydrate 0.097 g/100ml (25 °C)
Chromium oxalate 126 g/100 mL (0 °C)

to eliminate the excess oxalic acid that one would intentionally dump into the dissolved stainless steel, a solution of iron chloride would be added just until no more ppt forms, maybe a few drops excess iron chloride, the iron chloride would then with air react to ppt the iron chloride, leaving despite trace metals in stainless steel (manganese 0-2%, molybdenum, 316 SS?) a quite pure solution of chromium oxalate

i had previously thought about decomposing the whole lot of oxalates into corresponding oxides/hydroxides

iron oxalate as many know decomposes into nano iron metal, it then quickly reacts with air and moisture, it could possibly upon formation be removed per magnet assuming it would be fine powder, it does tend to form oxides and hydroxides upon decomposition however, not entirely pure iron powder.
nickel oxalate would decompose into quite pure nickel metal with trace amounts of nickel carbonate and hydroxide
chromium oxalate would decompose into Cr2O3 with CrO and Cr3O4 as intermediates (or the other way around) anyhow through decomposition of the metal oxalates it could be possible to dissolve the chromium oxides in strong alkali solution

now as i see it there is a chance of even dragging nickel and chromium somewhat unharmed out of stainless steel solution simply adding zinc, the iron would naturally through air exposure turn into hydroxides and oxide, a weak acid could be used to leech out the iron hydroxide, where Fe2O3 of what ive tried seems quite resistant to even HCl, nickel and chrome should dissolve a lot faster

"The highest chromium leaching was achieved with the aqueous solution of oxalic acid, as chromium was converted into water-soluble chromium oxalate."
http://agris.fao.org/agris-search/search.do?recordID=US20130...




~25 drops = 1mL @dH2O viscocity - STP
Truth is ever growing - but without context theres barely any such.

https://en.wikipedia.org/wiki/Solubility_table
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 13-5-2017 at 00:01


I'm going to work up some chromates that I produced in pretty much the same way with Ca(OCl)2 as soon as my new filter funnel arrives. One thing I have wondered about is whether it might be possible to leach chromium out of dissolved stainless steel using sodium hydroxide to make Na3Cr(OH)6.



View user's profile View All Posts By User
Antiswat
International Hazard
*****




Posts: 1234
Registered: 12-12-2012
Location: Dysrope (aka europe)
Member Is Offline

Mood: dangerously practical

[*] posted on 14-5-2017 at 01:12


i doubt that, 316 SS is resistant to boiling caustic soda, it tears only few millimetres per years exposure
electrolysis may be a thing, but im quite sure iron and nickel hydroxides will also be soluble




~25 drops = 1mL @dH2O viscocity - STP
Truth is ever growing - but without context theres barely any such.

https://en.wikipedia.org/wiki/Solubility_table
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 14-5-2017 at 01:25


The procedure would involve first dissolving the stainless steel in hydrochloric acid and then neutralizing with sodium carbonate.



View user's profile View All Posts By User
Antiswat
International Hazard
*****




Posts: 1234
Registered: 12-12-2012
Location: Dysrope (aka europe)
Member Is Offline

Mood: dangerously practical

[*] posted on 14-5-2017 at 02:14


thing is you get a mix of iron nickel and chromium carbonate/hydroxide
purity is the problem at that
you may try fractionally recrystallizing the NaCrO4 however
another way to get iron out of the mixed stainless chloride solution would be letting oxygen get at it, sadly it seems hydrogen peroxide wouldnt aid this reaction much as it would form actually more stable FeCl3, airbubbling the thing would be possible but still extremely messy and taking long time




~25 drops = 1mL @dH2O viscocity - STP
Truth is ever growing - but without context theres barely any such.

https://en.wikipedia.org/wiki/Solubility_table
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 14-5-2017 at 03:41


Nickel hydroxide is not soluble. Iron hydroxide is, but iron oxide is not. It could be tricky to remove all traces of iron that way; it would be easier to simply crystallize potassium dichromate, but with sodium hydroxide as the limiting reactant, I don't know if that would even be necessary.

No matter how you do it, it's going to be messy, but I think extracting with sodium hydroxide looks like a promising alternative that hasn't been tried by amateurs, and economy of reagents looks good that way.





View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*******




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 14-5-2017 at 17:33


Quote: Originally posted by JJay  
Nickel hydroxide is not soluble. Iron hydroxide is, but iron oxide is not. It could be tricky to remove all traces of iron that way; it would be easier to simply crystallize potassium dichromate, but with sodium hydroxide as the limiting reactant, I don't know if that would even be necessary.

I'm pretty sure that in the presence of oxygen, iron hydroxide forms iron oxide-hydroxide, which is that reddish-brown rust we all know and love. And that's quite insoluble in water. It might actually be easier than you think.
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 14-5-2017 at 19:01


I think you're right, and that process can be accelerated considerably by using hydrogen peroxide, which would also probably form insoluble iron (iii) oxide. I'm pretty sure there's also a risk of forming sodium ferrate this way, though.... It decomposes pretty easily, but I'm not 100% certain what the decomposition products are... iron (ii) hydroxide is the one to avoid... pretty sure iron (iii) hydroxide is insoluble.

[Edited on 15-5-2017 by JJay]




View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*******




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 15-5-2017 at 07:55


Quote:
I think you're right, and that process can be accelerated considerably by using hydrogen peroxide, which would also probably form insoluble iron (iii) oxide. I'm pretty sure there's also a risk of forming sodium ferrate this way, though.... It decomposes pretty easily, but I'm not 100% certain what the decomposition products are... iron (ii) hydroxide is the one to avoid... pretty sure iron (iii) hydroxide is insoluble.

Let's put it this way: it's much more likely that you form an iron iii compound when trying to get an iron ii compound or especially a ferrate than vice versa. If you did somehow get some in solution, it'd probably oxidize your chromium ions to hexavalent chromium, which would at least be very easy to notice.

I actually had a strip of spring steel that I'd dissolved in anoxic HCl some time ago, and I finally poured it out in a dish. The solution was a dull, dark blue-green color. I then added a solution of saturated sodium hydroxide, and if formed more of a sludge than a precipitate. I stirred it up, but nothing really settled. The color was more or less the same though. I noticed brown forming around the edges of the liquid, which was clearly iron oxide-hydroxide, so I dripped some 30% H2O2 in, and where each drop landed, a large brown spot formed. I then added quite a bit more, and stirred it up. A lot more of it turned brown, and that started to settle. The liquid above the settling brown rust precipitate was clear though, I'm not sure why that would be the case, and I can't test it until I get home from work.

edit: But I think it may be one of those dreaded double salts forming. Like chromite:

https://en.wikipedia.org/wiki/Chromite

It should at least be possible to concentrate in that state though.

[Edited on 5/15/17 by Melgar]
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 15-5-2017 at 13:19


The mixture containing the dissolved silverware that I have been playing with for a few weeks (so far it's been dissolved in HCl, precipitated out with sodium bicarbonate, washed, and reacted with bleaching powder) started to settle; it is still bubbling and smells like chlorine oxides, but the gas being emitted is definitely less noxious than before. The mixture will still need to be filtered, but I can see a dark orange solution above a dark brown/orange precipitate.

I'm pretty sure I'll get to it before this weekend.




View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*******




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 15-5-2017 at 13:43


Those orange-colored ones are usually nothing good: a combination of yellow iron chloride and reddish-brown oxide-hydroxide in various proportions, I bet.
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 15-5-2017 at 14:36


I'm sure the precipitate has nothing in it that I really want except for perhaps some nickel oxide. I think it's probably mostly iron oxide. Hopefully the vast majority of the chromium has leached out; my plan is to wash the precipitate until the washings turn clear and then put it in a trash bag, but if necessary I can add some hydrochloric acid and isopropyl alcohol and let it stand overnight (preferably outside). Then I'll just boil the washings / filtrate down in my 5L and collect crystal fractions before I decide what to do next. I'm tentatively leaning towards decomposing the calcium chlorates in a crucible and then making potassium dichromate, but I'd definitely prefer to have sodium dichromate....

[Edited on 16-5-2017 by JJay]




View user's profile View All Posts By User
battoussai114
Hazard to Others
***




Posts: 235
Registered: 18-2-2015
Member Is Offline

Mood: Not bad.... Not bad.

[*] posted on 15-5-2017 at 15:05


I think it was the materialsproject.org database that had pourbaix diagrams for multiple metal ions. You could use it to try and find conditions for precipitating one while leaving the other in solution.

[Edited on 15-5-2017 by battoussai114]




Batoussai.
View user's profile View All Posts By User
Antiswat
International Hazard
*****




Posts: 1234
Registered: 12-12-2012
Location: Dysrope (aka europe)
Member Is Offline

Mood: dangerously practical

[*] posted on 20-5-2017 at 00:36


hm hm.. nickel hydroxide should be possible to extract using ammonia, turning it into a complex, where iron shouldnt be very soluble with ammonia, essentially the solution could be evaporated off to take out the ammonia, until solution is almost entirely neutral which would make it unlikely for iron or chromium hydroxide to dissolve as they dont form water soluble compounds with ammonia, or are in general water soluble, only worry would be hydroxides gelling up

iron hydroxide regarded as soluble, isnt that only in strongly alkaline solutions? im seeing people suggesting its only "soluble" in acidic solutions, or in other words it isnt but its a base that can react with acids to form soluble compounds

i think its best avoided to deal with dichromate until you really want it, excess HCl can also form chlorochromate which over time and probably upon heating decomposes the HCl and chlorochromate into chlorine gas, very neat to have a bottle of, chlorine gas can be fun to play around with

on a sidenote the impure chromium hydroxide sludge can be added to electrolysis cell, a bit of iron will come out but for whatever uses chlorate has its merely benifitial to be contaminated with iron oxide




~25 drops = 1mL @dH2O viscocity - STP
Truth is ever growing - but without context theres barely any such.

https://en.wikipedia.org/wiki/Solubility_table
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 20-5-2017 at 01:02


My plan was to dissolve it in hydrochloric acid and crystallize it then heat it in a crucible to destroy any organics.

How could you not want dichromate?? It's extremely useful and interesting, not to mention recyclable. The downsides are a) it's toxic and b) it causes cancer, but I could say the same thing about 70% of my other chemicals.

On the other hand, I'm not really looking forward to filtering and boiling down 12L of calcium chromate solution to get 200 grams of crystals... but I am going to get started with that now....




View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 20-5-2017 at 01:37


IMG_20170520_013448[1].jpg - 447kB



View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 20-5-2017 at 22:29


So anyway, after many hours of boiling, washing, and filtration, I have about 4L of orange solution with some light precipitate starting to form in it. I'm not too sure about what that is, but I suspect it is calcium hydroxide or perhaps a basic calcium salt. There are also pine needles, metal oxides, and other undesirable solids floating around since a lot of the mixture was just decanted and not filtered. The washings from the metal sludge are now yellow. The theoretical yield is 244 grams, which would require about 1.5 liters of water to dissolve fully, but there is likely a lot of dissolved calcium chloride and some calcium chlorate, which decrease the solubility of calcium chromate, although to what degree I do not know. My plan now is to continue washing chromates out of the sludge with water until I get bored doing that and then try to filter the sludge and neutralize any remaining oxidizers with sodium bisulfite. Then I'll evaporate the filtrate down to oh I dunno... maybe 2.5L, filter it, and then start collecting crystal fractions maybe every 500 mL or so, cooling the beaker to room temperature in an ice bucket before filtering fractions. Either that or I'll just evaporate off all the water and put the experiment on the shelf since this takes a lot of time and produces a common reagent, although it is fun IMHO.

[Edited on 21-5-2017 by JJay]




View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 22-5-2017 at 05:05


After doing some filtering and whatnot, I now have about 2.5L of orange solution. I thought it looked a little bit dingy, so I added a little hydrogen peroxide to see what would happen. The solution immediately turned completely brown/black and started fizzing. The color was reminiscent of a manganese compound. Over time, it gradually returned to a brighter orange.

I'm a little unsure about what the black color could have been, but I have seen it before with hydrogen peroxide when trying to recycle chromium waste (which should have contained few mineral impurities, but it's hard to say 100% for sure). At this point, I'm not certain that this isn't some impurity. I can't 100% for sure rule out the presence of manganese chloride, but I think it is unlikely that any is present.

I'm picking up some lab grade sodium chromate later and will see if it has a similar reaction with hydrogen peroxide.

IMG_20170521_225357[1].jpg - 391kB

[Edited on 22-5-2017 by JJay]




View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 22-5-2017 at 10:10


The first crystal fraction (everthing above 2000 mL) contains a significant amount of yellow powder and some flat square-shaped crystals. The yellow powder I think formed as the water boiled off and the crystals I think formed as the solution cooled. As is typical of mixtures containing calcium salts, the mixture is hard to filter. I don't know for sure yet how pure it is, but indications are that the filter cake consists largely of calcium chromate.



View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*******




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 22-5-2017 at 10:22


Lots of transition metal ions will catalyze the decomposition of H2O2, iron being one of them. Are you familiar with Fenton's reagent and Fenton chemistry?

Anyway, yellow is far more likely to be an iron iii salt I think. They're very persistent. And very yellow.
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 22-5-2017 at 10:37


I don't see why iron iii would be crystallizing out at this point unless there happened to be an extremely large amount of it in solution, which is extremely unlikely, and it makes sense for calcium chromate to be crystallizing about now. Actually, I think the suggestion that the precipitate is iron(iii) is preposterous, and if you're making outlandish suggestions for pedagogical reasons, please desist - that's not actually good pedagogy. But traces of iron compounds (likely present) might turn black with peroxide....

Obvious checks include testing its solubility both before and after heating at high temperatures, seeing if a solution produces a precipitate and a red color with sulfuric acid, etc. But I'm going to collect all of the fractions before I do that.




View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 22-5-2017 at 11:24


I have very little information on manganous chromate, but this dialog suggests that it is sparingly soluble in water. Its presence in chromate salts would almost certainly be undesireable: https://books.google.com/books?id=Nxw_AQAAMAAJ&pg=PA94&a...





View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*******




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 22-5-2017 at 11:30


Just saying that from my own experience trying to separate nickel from stainless steel, getting rid of the iron salts was very difficult. It didn't help that chromium can also be green, and mixed iron salts can be sort of green especially with ammonium present.

Also, white crystals forming in a strongly colored solution will often take on some color from the solution and need additional recrystallization to purify completely.
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 22-5-2017 at 12:02


There could be and likely is some calcium hydroxide precipitating, but keep in mind that calcium chromate is a very yellow pigment sometimes referred to as Yellow 33; while it's been largely phased out due to both toxicity and in favor of more chemically resistant pigments like lead chromate and cadmium chromate, it is still used in oil paints and wood stains. I'm not personally planning on using it as a pigment, but I do know an artist who wants some and thinks it is super cool that it is made out of silverware...



View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3321
Registered: 15-10-2015
Member Is Offline

Mood: resigned

[*] posted on 22-5-2017 at 14:53


Fraction 1. It is extremely bright yellow and sparkly with the consistency of fine sand, and given the conditions under which it was produced, I am sure that it is substantially calcium chromate. I can tell it is not quite pure... it contains some pale amorphous material and square crystals, and the square crystals are actually white. I'm not 100% sure what the impurities are, but my guess would be calcium hydroxide, which might explain why this was so hard to filter. I'll have to dry everything out before I weigh it, and a recrystallization is certainly called for, but it looks like there are 50-100 grams here.

IMG_20170522_144237[1].jpg - 500kB





View user's profile View All Posts By User