I was just wondering if there is a way to recover either nickel or chromium from a solution of nicrome wire in some acid.. i have no nickel or chrome
compounds yet and was about to throw out all my excess bits of the wire so i thought id ask. all the best folks.
|
|
|
not_important
International Hazard
   
Posts: 3873
Registered: 21-7-2006
Member Is Offline
Mood: No Mood
|
|
Perhaps the most economical would be to add alkaline peroxide and boiling, Ni should drop out as oxides while Cr would stay in solution as chromate.
|
|
|
Mumbles
National Hazard
  
Posts: 436
Registered: 12-3-2003
Location: US
Member Is Offline
Mood: Procrastinating
|
|
In a solution addition of iron will precipitate the nickel but not the chromium. I'd add some NaOH to the solution to neutralize any remaining acid.
The NaOH won't redissolve the nickel.
|
|
|
12AX7
Post Harlot
   
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
Precipitating it all as hydroxide or, cheaper, carbonate, and fusing with alkali and oxidizer may be a better route to seperating the chrome.
You may be able to plate the nickel out electrolytically in an acid solution. Chromium would be less preferred because it would tend to react with
the acid and nickel. A seperate anode cell may be wanted, otherwise you'll get a bunch of chlorine or something.
Edit: And, you can always synthesize a pound of methylglyoxime, precipitate the nickel, filter, and either ash or acidify the complex to free the pure
nickel.
Tim
[Edited on 3-24-2007 by 12AX7]
|
|
|