Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: Removing Lime deposits from Copper kettle
dann2
International Hazard
*****




Posts: 1523
Registered: 31-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2008 at 11:54
Removing Lime deposits from Copper kettle


Hi,

I have a kettle made from Copper that needs the Lime removed from it. (the Lime has build up from hard water deposits).
I have seen Citric acid and Formic acid used for descaling Kettles but these attack the Copper.
Can anyone recommend something which will attack the Lime but not the Copper.
One (perhaps barmy) idea I have had was to add Sulphuric acid to the Kettle and using a Graphite rod connect a power supply to the Kettle + Grahpite thus cathodically procecting the Kettle. You could heat the acid to make it work faster. The Lime deposits are very hard and stubborn.

Dann2
View user's profile View All Posts By User
DJF90
International Hazard
*****




Posts: 2266
Registered: 15-12-2007
Location: At the bench
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2008 at 12:16


Lime (CaCO3) does not react well with sulphuric acid, as in my experience a protective layer of insoluble calcium sulphate stops the rest of the lime reacting. HCl would likely be a better choice, as it should not react with the copper metal (as copper is below hydrogen in the reactivity series, and there is no oxidiser present).
View user's profile View All Posts By User
kclo4
National Hazard
****




Posts: 916
Registered: 11-12-2004
Location:
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2008 at 13:07


Last time I checked Vinegar doesn't react with copper metal, It will take off any oxide making it look bright pink.

Calcium, and Magnesium Acetate are also very soluble so you wouldn't have the problem H2SO4 gives you.

I would make sure it isn't touching any other metal however. I mixed vinegar with salt and it started to dissolve some copper around the edge of a penny where the zinc was exposed. I'm pretty sure this was some sort of electrochemical reaction.
View user's profile Visit user's homepage View All Posts By User
chemkid
Hazard to Others
***




Posts: 269
Registered: 5-4-2007
Location: Suburban Hell
Member Is Offline

Mood: polarized

[*] posted on 14-9-2008 at 13:44


HCl pretty simple...barely reacts with copper and will take only a few seconds to work



View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 14-9-2008 at 15:27


Let's see here...

HCl: complexes copper. Dang. (Probably not an issue at dilute strength though.)
Acetic acid: complexes copper. Dang.
Sulfuric acid: leaves copper alone, but doesn't dissolve calcium real great. Dang.
Nitric acid: strong oxidizer...but only when strong. Dilute HNO3 (5%?) should work perfectly, no? :)

Does formic acid complex transition metals? I see a few journal hits for "formatocopper", so I guess it exists under some conditions at least.

Smooth off the copper with a scrub pad when you're done. A little acid won't hurt anything, but it will leave a matte surface prone to corrosion. Oh, and a dash of oil rubbed on when you're done to keep it shiny. Then hang it on the wall, because copper is almost too beautiful to use. :D

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
chloric1
International Hazard
*****




Posts: 1179
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline

Mood: Stoichiometrically Balanced

[*] posted on 14-9-2008 at 16:24


I am going for a stretch here but....how about NO acid?! I am thinking chelating agents here. A couple suggestions:

Tetrasodium EDTA or other EDTA
Sodium Citrate
Tetrapotassium pyrophosphate
Sodium Tripolyphosphate
Sodium gluconate with a little NaOH

All easily had from ebay and will not oxidize copper metal.




Fellow molecular manipulator
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 14-9-2008 at 16:36


EDTA crossed my mind, but how well does it complex calcium, and how quickly? Could be soaking for a while. In the mean time, oxygen is going to work on the copper. I think the solution will inevitably turn green (or blue or whatever), it's just to what degree.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
dann2
International Hazard
*****




Posts: 1523
Registered: 31-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2008 at 16:44


Thanks alot for the responses.
I used 12% HCl. Builders store for cleaning cement. Worked very fast and I got no blue colour so it did not attack the Copper.

Formic acid (I tried it) does give a blue colour. It was 100% stuff though.

Dann2
View user's profile View All Posts By User
The_Davster
A pnictogen
*******




Posts: 2861
Registered: 18-11-2003
Member Is Offline

Mood: .

[*] posted on 14-9-2008 at 16:53


I think this is being overcomplicated

HCl

It takes time for enough oxygen to dissolve in HCl to even notice colouring of the solution with green CuCl4(2-). And if you are still worried add a little sulfite or thiosulfite as a reducing agent to the solution.

Just fill the kettle, and stopper to prevent air from entering.
After lime has dissolved rinse well and oil




View user's profile View All Posts By User
ScienceSquirrel
International Hazard
*****




Posts: 1863
Registered: 18-6-2008
Location: Brittany
Member Is Offline

Mood: Dogs are pets but cats are little furry humans with four feet and self determination! :(

[*] posted on 14-9-2008 at 17:16


Sulphamic acid is pretty juicy stuff.

It is the basis of a lot of descaling materials.
View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 15-9-2008 at 12:07


@dann2: I like the idea of trying galvanic protection. You can test whether it works with a piece of copper wire in your cleaning solution. Look for a mass difference in the test piece before or after.

As for a chemical, just try a commercial vendor. One I use is CLR Calcium-Lime-Rust Remover. Its MSDS lists its active ingredients. Here's the manufacturer Jelmar's MSDS page. It's currently listed acids are lactic and gluconic.

(Aside @ScienceSquirrel. I believe CLR used to contain sulphamic acid.)

I also might point out that regardless of your cleaning method, you can always plate new copper on. Right after cleaning, that base surface should be right ready to go. Since you're only cleaning the inside of a vessel, you can use that same vessel to hold your plating solution. In other words, since you don't need to plate the outside, don't try.
View user's profile View All Posts By User
chloric1
International Hazard
*****




Posts: 1179
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline

Mood: Stoichiometrically Balanced

[*] posted on 15-9-2008 at 13:11


I don't necessarily think I am trying to overcomplicate things just wanted to offer a nonaggresive form of lime removal. The chelating agents I referred to, especially polyphosphate, have specific activity towards calcium and magnesium. I was thinking that dann2 would be able to use reagents I mentioned without comprising any natural patina that might be on the pot. Some copper items are better off brown, green or whatever.



Fellow molecular manipulator
View user's profile View All Posts By User
argyrium
Hazard to Others
***




Posts: 123
Registered: 3-2-2008
Location: Pacific
Member Is Offline

Mood: No Mood

[*] posted on 16-9-2008 at 11:13


chloric1 is correct in his post concerning Na polyphosphate for a non aggressive/conservative treatment that would do little damage to the patina on Cu (or bronze/brass).

The commercially available product, Calgon (NaPO3)x at 5 - 15% in water can do pretty amazing things to calcareous deposits if allowed to soak - sometimes for days.

Alkaline Rochelle salts and alkaline (NaOH) glycerine can also be quite effective, but slower still.