Perfluorpolyeter


Perfluorpolyeter is used in vapour phase reflow soldering because of being inert up to high temperatures. It is sold by, for example, Imides,

who described it as

CF3 – O – CF – CF2 – O – CF – CF2 – O – CF – CF2 – O – CF – CF2 – ……………… – O – CF3 CF3 CF3 CF3 CF3

"The liquid polymers of the Galden FM series are built according to this principle."

Does this structure make any sense? Can you have "– CF2 – O – CF – CF2 – ".

If anyone can make a drawing in for example ACD/ChemSketch and share the file that would be great.


If anyone is interested in how the substance is used in the DIY manufacturing of PCBs, watch

https://youtu.be/D28uSzCs7-k?t=620
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4687
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: Preparing to defend myself (academically)

[*] posted on 8-5-2021 at 12:06


I would expect that all the CF3s listed at the end there are supposed to be attached to the CFs, since -CF- is missing one substituent.



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
JohnnyBuckminster
Harmless
*




Posts: 40
Registered: 6-6-2018
Member Is Offline


[*] posted on 8-5-2021 at 19:07


Ok, that make sense. The extra CF3's at the end should be attached to the -CF- groups, like in the image below.



screenshot.png - 3kB
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4687
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: Preparing to defend myself (academically)

[*] posted on 8-5-2021 at 19:16


Exactly!



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
Dr.Bob
International Hazard
*****




Posts: 2838
Registered: 26-1-2011
Location: USA - NC
Member Is Offline

Mood: Mildly disgruntled scientist

[*] posted on 10-5-2021 at 10:30


That makes sense, likely made from hexafluoropropene (a cheap byproduct of Teflon production), which would be epoxidized and then polymerized. Short chains of this are used as solvents for PTFE production and considered long lasting enviromental issues.
View user's profile View All Posts By User
JohnnyBuckminster
Harmless
*




Posts: 40
Registered: 6-6-2018
Member Is Offline


[*] posted on 11-5-2021 at 11:39


In the Hydrogen–deuterium exchange process covalently attached hydrogens are replaced with deuterium over time, I read this in Wikipedia.

Would a similar approach work to manufacture hexafluoropropylene, i.e exposing propylene to an excess of fluoride ions over time? Would the hydrogen spontaneously be replaced with fluoride, like in the scheme below?

screenshot.10.png - 4kB
View user's profile View All Posts By User
DraconicAcid
International Hazard
*****




Posts: 4429
Registered: 1-2-2013
Location: The tiniest college campus ever....
Member Is Offline

Mood: Semi-victorious.

[*] posted on 11-5-2021 at 11:50


I very seriously doubt it.



Please remember: "Filtrate" is not a verb.
Write up your lab reports the way your instructor wants them, not the way your ex-instructor wants them.
View user's profile View All Posts By User
Dr.Bob
International Hazard
*****




Posts: 2838
Registered: 26-1-2011
Location: USA - NC
Member Is Offline

Mood: Mildly disgruntled scientist

[*] posted on 11-5-2021 at 13:01


There are electrochemical ways to swap F for H, but they are not trivial, mostly done on industrial scale.

Fluoride ions are not likely to displace hydride from a hydrocarbon.

But you can make perfluoropropane by fluoronating perfluoropropylene, using CoF3 as the fluorinating material. Exposing propylene to straight fluorination would likely create a large explosion.