Reduction of Mn oxides with C to Metallic Mn


Im trying to get metallic Manganese for electrolisis.
(actually Im testing electrollitical Mn form MnSO4) with more or less success.

From the Wiki:

MnO2 + C → Mn + CO2

I ve some Mn oxides (high oxides) left from battery leachings for getting MnSO4.

I follow Der Alte procedure in which you burn battery MnO2 to get Mn2O3 for futher processing.

"(B1) For Zn/C cells only: put in a tin can and heat to bright red heat. All MnO2 will convert to Mn2O3 @ 700C+ and the carbon should burn off; also zinc/ammonia complexes will drive off ammonium chloride as white clouds and worry the neighbors. Cool, treat with cold dilute acid (N/10 or less) to get rid of any ZnO. Pour off acid, and wash. Complex but unless carried out the product will be polluted. Resultant should be mainly Mn2O3: go to step (C)"

So the questions:

1) Is this reduction posible as for an amateur?
2) Which temperature should a mix of Carbon and MnOx used to get the reduction?

from this paper state 27 to 1227°C (pressure related)

3Mn2O3 + C = 2Mn3O4 + CO (ΔGo = - 0.25 ? 0.17T 25°-1100°)
Mn3O4 + C = 3MnO + CO (ΔGo = 110.96 ? 0.21T 25°-1244°
ΔGo = 84.35 ? 0.20T 1244°-1700°
MnO + C = Mn + CO (ΔGo = 287.6 ? 0.16T 25-1227°)

(NOTE: i do not understand this free gibs, but probably you do.)

https://www.alliedacademies.org/articles/practical-reduction...

3) the procedure should be as simple as : add MnOx + C in a tin can (close or not) and heat to 1300°C?

(NOTE: I will need manganese metal for electrolitic KMnO4 production, so the least contamination of other metals - so thermite is no good)

also there is the dicotomy from Der Alte: " 700C+ and the carbon should burn off;" and "I need the carbon for the reduction"

4) "Dont go this route and keep your electrolythical method"....

thanks








Go SAFE, because stupidity and bad Luck exist.
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10553
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 3-3-2023 at 10:28


Quote: Originally posted by RU_KLO  

(NOTE: I will need manganese metal for electrolitic KMnO4 production, so the least contamination of other metals - so thermite is no good)



Thermite can produce very pure metals but the MnO2 thermite is very low yield because the boiling point of Mn is about the same as the melting point of alumina. This causes the Mn to largely boil off.

Because these carbothermic reductions are so endothermic, very high temperatures are needed (see Ellingham diagrams)