Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: Low solubility tin salts?
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 9-4-2024 at 03:16
Low solubility tin salts?


Hi all, I have been attempting to refine relatively pure tin based on a procedure explained in https://www.sciencemadness.org/whisper/viewthread.php?tid=14...

My cell operated well at about 2v for almost 2 weeks and I generated about 150g of tin crystals during that time. The electrolyte was 20g/L SnCl2 and a fair bit of HCl (not sure of the concentration of HCl but the electrolyte had a PH of about 2 according to some cheap test strips for soil that I used). The anode was cast from an old pewter mug from an op shop (marked as lead free) and the cathode was 316 stainless. As the anode was corroded, black mud formed on it which I scraped off and put aside. I am unsure of the composition of it, but I suspect it contains antimony and copper as they are common alloying elements in pewter. After almost 2 weeks working well, I left the cell running for a couple of hours and when I came back the electrolyte had formed an off-white suspension of something that obviously has a low solubility and no more tin was plating out. I let the electrolyte dry out for about a month and a substantial amount of a whitish substance with no visible crystal structure has deposited in the bottom of the cell. Any ideas on what happened or what the substance is?

3217E0DE-9D3A-4766-A63A-6516655284A7.jpeg - 3MB 3217E0DE-9D3A-4766-A63A-6516655284A7.jpeg - 3MB B9552CCB-28F1-4590-B0E7-5404A3027E84.jpeg - 2.4MB

[Edited on 9-4-2024 by currawong]
View user's profile View All Posts By User
RU_KLO
Hazard to Others
***




Posts: 318
Registered: 12-10-2022
Location: Argentina
Member Is Offline


[*] posted on 9-4-2024 at 07:36


if it is "whitish" insoluble, probably tin oxide (SnO2).




Go SAFE, because stupidity and bad Luck exist.
View user's profile View All Posts By User
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 9-4-2024 at 12:21


Tin oxide sounds plausible, any idea how it formed? If it is tin oxide, could it be converted back into tin metal by dissolving it in nitric acid and precipitating tin metal powder with a less nobel metal eg zinc? No idea if that would work, I am still learning and would appreciate any advice.
View user's profile View All Posts By User
Lionel Spanner
Hazard to Others
***




Posts: 203
Registered: 14-12-2021
Location: near Barnsley, UK
Member Is Offline


[*] posted on 9-4-2024 at 14:49


The typical way to reduce tin oxide to metallic tin is to heat it with carbon.

There may well be solution-based methods, but they appear to be pretty obscure.




Industrial chemist rediscovering the practical pleasures of pure chemistry.
Sometimes I make videos - https://www.youtube.com/@yorkshirechemist
View user's profile View All Posts By User
Rainwater
National Hazard
****




Posts: 993
Registered: 22-12-2021
Member Is Offline

Mood: Break'n glass & kick'n a's

[*] posted on 9-4-2024 at 15:12


It sounds like the ph of the cell got to high. You can take a sample of the unknown and try to react it with fresh HCl, if it is tin oxide it should go back into solution
Post/preview edit:
If it does not dissolve, test for AgCl.
take another sample and add more than 1/3 its weigh NaOH. It should turn dark gray / black. heating may be required on small scale. >=80c
Then add an equal wight of corn syrup.( major excess for faster results)
A silvery percipitate will form.

[Edited on 9-4-2024 by Rainwater]




"You can't do that" - challenge accepted
View user's profile View All Posts By User
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 9-4-2024 at 15:35


Tin oxide melts at 1600 degrees Celcius, so with my setup I don't think carbon reduction is practical. I am also interested in the black anode slime because I tried to melt a piece of it with a blowtorch and tiny silver beads appeared on the surface.
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3938
Registered: 8-2-2015
Member Is Offline


[*] posted on 9-4-2024 at 15:50


When dissolving solid tin in hydrochloric acid with no stirring, over days,
after a while, surrounding the tin, a black 'cloud' appears.
Swirling/mixing quickly dissolves the black cloud.
(I suspect titny tin particles in depleted acid,
swirling mixes particles and acid with rapid reaction,
just a guess/idea) .
Anyway, tiny particles of metal in suspension or wet, often look black.




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 9-4-2024 at 16:11


Thanks Sulaiman, I noticed those black particles when making SnCl2 for the cell at the start. I used 10g lead-free solder that was 97% pure tin and 3%Ag and it took about a week to dissolve at room temp. For me though the black particles did not dissapear with stirring or the addition of small amounts of fresh acid so I filtered them out before starting the cell.

Rainwater, Thanks for your suggstions, I will definitely try both procedures when I get home. Is corn syrup the same as glucose syrup? I have not seen corn syrup sold in Australia.
The dark grey precipitate you are describing would be Sn(OH)2, correct?
View user's profile View All Posts By User
Rainwater
National Hazard
****




Posts: 993
Registered: 22-12-2021
Member Is Offline

Mood: Break'n glass & kick'n a's

[*] posted on 9-4-2024 at 16:41


Corn syrup is glucose and dextrose i think. Not sure which one is the reducing sugar, but thats the one you need.... googling.... glucose
Another test for AuCl is its exothermic reaction with powdered aluminum. But you need a good amount and its an expensive flash
https://youtu.be/Rvq3LjHJvsM?si=IyoE2vUXdlCGz3Ax

Quote:
The dark grey precipitate you are describing would be Sn(OH)2, correct?
Silver oxide.
Silver + HCl makes a white fluffy cloud in solution, and is a common alloy in your starting materials.
I extract silver from copper (brazed and soldered) joints by using the scrap as a anode in an hcl solution. Your description and starting materials are a perfect match.
If you follow mysteriusbhoice instructions here, and use this membrane as a filter for your anode, you will contain all the "slimes" for latter processing, while extracting a more pure tin product

[Edited on 10-4-2024 by Rainwater]




"You can't do that" - challenge accepted
View user's profile View All Posts By User
bnull
National Hazard
****




Posts: 985
Registered: 15-1-2024
Location: East Woods
Member Is Offline

Mood: Allergic

[*] posted on 9-4-2024 at 18:17


Quote: Originally posted by Rainwater  
If it does not dissolve, test for AgCl.
take another sample and add more than 1/3 its weigh NaOH.

You can also try ammonium hydroxide. If it dissolves, it's AgCl, and you can use a reducer like formaldehyde or glucose to precipitate silver.

AgCl darkens when left under UV light or sunlight.




Quod scripsi, scripsi.

B. N. Ull

We have a lot of fun stuff in the Library.

Read The ScienceMadness Guidelines. They exist for a reason.
View user's profile View All Posts By User
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 10-4-2024 at 01:57


Thanks again Rainwater, I added about 0.2 g of the white substance to 10 ml 32% HCl and it dissolved quickly. I also did a control with plain water and it did not dissolve as expected which would lead me to conclude that it is tin oxide. On the weekend when I have some more time I will try to restart the cell by adding more HCl and post an update here.

[Edited on 10-4-2024 by currawong]
View user's profile View All Posts By User
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 10-4-2024 at 02:09


Quote: Originally posted by Rainwater  
Corn syrup is glucose and dextrose i think. Not sure which one is the reducing sugar, but thats the one you need.... googling.... glucose
Another test for AuCl is its exothermic reaction with powdered aluminum. But you need a good amount and its an expensive flash
https://youtu.be/Rvq3LjHJvsM?si=IyoE2vUXdlCGz3Ax

Quote:
The dark grey precipitate you are describing would be Sn(OH)2, correct?
Silver oxide.
Silver + HCl makes a white fluffy cloud in solution, and is a common alloy in your starting materials.
I extract silver from copper (brazed and soldered) joints by using the scrap as a anode in an hcl solution. Your description and starting materials are a perfect match.
If you follow mysteriusbhoice instructions here, and use this membrane as a filter for your anode, you will contain all the "slimes" for latter processing, while extracting a more pure tin product

[Edited on 10-4-2024 by Rainwater]


That is really interesting, I attempted the same project where I melted down 300g of silver brazed copper joints into a slab of copper and dissolved it as the anode in an attempt to get a few grams of usable silver metal but I used sulphuric acid instead of hydrochloric and all I managed to do was make a lot of copper sulphate to the point where it was a saturated solution and it was crystalising out. I diddnt observe any anode slime so I assumed that there must have been very little silver in the brazing alloy used. What would be your advice on what to do with the anode slime from my tin refining? I have about 40g of it and it would be a fun project to get some relatively pure antimony for the element collection.
View user's profile View All Posts By User
Rainwater
National Hazard
****




Posts: 993
Registered: 22-12-2021
Member Is Offline

Mood: Break'n glass & kick'n a's

[*] posted on 10-4-2024 at 02:45


I dont know about antimony.
But assuming you have antimony, silver, copper, nickel and lead alloy, i start by electrolysis in hcl with an stainless steel cathode. Bag the anode basket.
The slimes are dried and refluxed in a solution of nitric acid.
Filtrate is used for selective percipitation.

Hold on...
I copy sreetips on youtube




"You can't do that" - challenge accepted
View user's profile View All Posts By User
AgCollector
Harmless
*




Posts: 26
Registered: 31-7-2018
Member Is Offline


[*] posted on 24-5-2025 at 15:20


Quote: Originally posted by currawong  
Thanks again Rainwater, I added about 0.2 g of the white substance to 10 ml 32% HCl and it dissolved quickly. I also did a control with plain water and it did not dissolve as expected which would lead me to conclude that it is tin oxide. On the weekend when I have some more time I will try to restart the cell by adding more HCl and post an update here.

[Edited on 10-4-2024 by currawong]


Based on your description it sounds like the white substance is the hydrolysis product of tin(II) when not enough HCl is in solution - i.e. the equilibrium went to the right:

SnCl2(aq) + H2O(l) -> Sn(OH)Cl(s) + HCl(aq)

which then shifted back left to dissolve when HCl was added.
View user's profile View All Posts By User
AgCollector
Harmless
*




Posts: 26
Registered: 31-7-2018
Member Is Offline


[*] posted on 24-5-2025 at 15:29


Quote: Originally posted by currawong  

...What would be your advice on what to do with the anode slime from my tin refining? I have about 40g of it and it would be a fun project to get some relatively pure antimony for the element collection.


In my experience this slime contains all the lead, antimony, and copper originally present in the pewter, plus a good deal of unoxidized tin too. I started playing around with separating them by reacting with concentrated HCl + H2O2 where initially only PbCl2 is present in the precipitate, then if you lower the HCl concentration a little antimony hydrolysis products come out too (Sb + O(H?) + Cl) but this precipitate is more gooey & soft and also keeps a lot of solution with it, bringing a lot of Sn & Cu with it too. It can be washed out with repeated ~1 M HCl rinsing but I didn't do anything more with it after that. If you wanted to try to isolate Sb though I'd suggest this route to eventually get Sb2O3 which could then be reduced.
View user's profile View All Posts By User
currawong
Harmless
*




Posts: 33
Registered: 9-4-2024
Location: Australia
Member Is Offline


[*] posted on 25-7-2025 at 17:27


Thanks AgCollector, I apologise for the long delay in responding. I really appreciate input from the original author of this method and I plan to start up the cell again sometime soon after my exams are finished. I still have the anode slimes and I will try rinsing them with HCl. Might also be worth trying to melt it in an inert atmosphere if it has a lot of unoxidised tin present to get a new anode plate.
View user's profile View All Posts By User

  Go To Top