making zinc powder form zinc sulfate
extraction is electrolytic. Dissolution of crude zinc oxide, ZnO, in sulfuric acid gives zinc sulfate, ZnSO4 in solution. Electrolysis of the ZnSO4
solution using aluminum cathodes and lead alloyed with silver anodes gives pure zinc metal coated on the aluminum. Oxygen gas is liberated at the
anode.
sulfuric acid is also made in this process and is recycled to dissolve more zinc oxide forming zinc sulfate
well i have a platinum anode so i don't want to mess with lead
and aluminum cathode easy to find any one know if the zinc will react with very dilute sulfuric acid im guessing the reaction is like copper sulfate
and maybe the aluminum cathode gets consumed if they are in all the same electrolyte
i guess i could just use a salt bridge
melting points
680 ºC decomp. (anhydrous)
100 °C (heptahydrate)
70 °C, decomp (hexahydrate)
http://www.webelements.com/zinc/
both 1 pound
>zinc powder
$12.44
$17.44 with tax and shipping
>zinc sulfate
$3.99
$9.99 with tax and shipping
and sulfuric acid can be recovered from it
and 5 pounds zinc sulfate
$10.99
$21.99 with tax and shipping
[Edited on 20-4-2011 by symboom]
|
|
|
Bot0nist
International Hazard
   
Posts: 1559
Registered: 15-2-2011
Location: Right behind you.
Member Is Offline
Mood: Streching my cotyledons.
|
|
Zinc is less than half the weight of the compound zinc sulfate. It would almost be worth it fiscally if not for the investment in time(lots) and
equipment. Still it would be fun though.
[Edited on 20-4-2011 by Bot0nist]
U.T.F.S.E. and learn the joys of autodidacticism!
Don't judge each day only by the harvest you reap, but also by the seeds you sow.
|
|
|
symboom
International Hazard
   
Posts: 1145
Registered: 11-11-2010
Location: Wrongplanet
Member Is Offline
Mood: Doing science while it is still legal since 2010
|
|
i would more do it for the experience and the got to at least try it once. ill probably do it using a salt bridge just to be safe
last thing i want is just a bunch of H2 and O2 and no product
|
|
|
roamingnome
Hazard to Others
 
Posts: 363
Registered: 9-9-2006
Member Is Offline
Mood: No Mood
|
|
this sounds real cool
with enough zinc you could make your self an electric car
and with enough renewable energy you can recycle the oxidized zinc.
|
|
|
symboom
International Hazard
   
Posts: 1145
Registered: 11-11-2010
Location: Wrongplanet
Member Is Offline
Mood: Doing science while it is still legal since 2010
|
|
my idea was more as using it to reduce MnO2 forming a slow thermite that is normally energetic and fast burning
Zn/MnO2 thermite
and for other pyrotechnics instead of using it in a disposable recyclable battery for an electric car and recycling the zinc oxide
but i guess the sky is the limit
|
|
|
redox
Hazard to Others
 
Posts: 268
Registered: 22-2-2011
Location: The Land of Milk and Honey
Member Is Offline
Mood: Chalcogenetic
|
|
I think (maybe I'm wrong) that you could simply add a piece of aluminum foil to the zinc sulfate solution. The aluminum would displace the zinc giving
aluminum sulfate and zinc metal. It might take a while though.
|
|
|
Bot0nist
International Hazard
   
Posts: 1559
Registered: 15-2-2011
Location: Right behind you.
Member Is Offline
Mood: Streching my cotyledons.
|
|
| Quote: | | **- add a piece of aluminum foil to the zinc sulfate solution. |
Works with a CuSO<sub>4</sub>-5H<sub>2</sub>O solution to get Cu. Pretty violently in fact.
[Edited on 22-4-2011 by Bot0nist]
U.T.F.S.E. and learn the joys of autodidacticism!
Don't judge each day only by the harvest you reap, but also by the seeds you sow.
|
|
|
Random
International Hazard
   
Posts: 1120
Registered: 7-5-2010
Location: In ur closet
Member Is Offline
Mood: Energetic
|
|
I tried putting Al into CuCl2 and it was violent reaction while putting Al into ZnCl2 didn't even cause reaction (or maybe it was very slow).
|
|
|
symboom
International Hazard
   
Posts: 1145
Registered: 11-11-2010
Location: Wrongplanet
Member Is Offline
Mood: Doing science while it is still legal since 2010
|
|
that's interesting. Aluminum is used as the cathode i would thought it would be noticeable reaction. maybe could be the same with some other elements.
|
|
|
Neil
National Hazard
  
Posts: 556
Registered: 19-3-2008
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Bot0nist  | | Quote: | | **- add a piece of aluminum foil to the zinc sulfate solution. |
Works with a CuSO<sub>4</sub>-5H<sub>2</sub>O solution to get Cu. Pretty violently in fact.
[Edited on 22-4-2011 by Bot0nist] |
I've never managed to get that to work without adding a Chloride salt. Did you heat the mixture?
Zn and Al form some interesting intermetallics. If you get a nice coating of fine Zn powder all over the Al, I wonder if heating would be enough to
trigger a reaction. I have a feeling it would end up being too passivated with aluminum hydroxide goo. there is a phase diagram on page 27 of a Al/Zn
system. http://books.google.ca/books?id=Uimniogb0DEC&pg=PA25&...
[Edited on 4-5-2011 by Neil]
|
|
|
symboom
International Hazard
   
Posts: 1145
Registered: 11-11-2010
Location: Wrongplanet
Member Is Offline
Mood: Doing science while it is still legal since 2010
|
|
my guess is the aluminum is has Cathodic protection and is slightly more reactive than zinc (zinc oxide and aluminum thermite shows this)once power is
turned off a battery effect might form as the aluminum becomes the anode in the battery and the platinum the cathode.
|
|
|
Bot0nist
International Hazard
   
Posts: 1559
Registered: 15-2-2011
Location: Right behind you.
Member Is Offline
Mood: Streching my cotyledons.
|
|
Quote: Originally posted by Neil  | Quote: Originally posted by Bot0nist  | | Quote: | | **- add a piece of aluminum foil to the zinc sulfate solution. |
Works with a CuSO<sub>4</sub>-5H<sub>2</sub>O solution to get Cu. Pretty violently in fact.
[Edited on 22-4-2011 by Bot0nist] |
I've never managed to get that to work without adding a Chloride salt. Did you heat the mixture?
[Edited on 4-5-2011 by Neil] |
Sorry, I always add NaCl also. Off topic, but the resulting Cu formed can be easily powdered when dry and makes an amazing flash with
KClO<sub>3</sub> a touch of sulfur to get it to take flame.
U.T.F.S.E. and learn the joys of autodidacticism!
Don't judge each day only by the harvest you reap, but also by the seeds you sow.
|
|
|
AJKOER
Radically Dubious
   
Posts: 3026
Registered: 7-5-2011
Member Is Offline
Mood: No Mood
|
|
It turns out that the Al and CuCl2 is a known and as of yet, not completely understood reaction as to the mechanics of exactly why it proceeds so
vigorously (other than the protective Al2O3 coating is effectively removed).
My hint of the day is to prime the Al surface by pre-soaking in Acetic acid followed by thorough rinsing. Even if there is no apparent reaction, give
it 8 hours at room temperature (or heat it to speed things up). Unexpectedly, this priming works in trying to dissolve Al foil in NH4OH that otherwise
remains unreactive (this is an experiment that I have performed based on an article by a Al coating manufacturer noting the ability of Acetic acid to
disrupt the protective coating).
Good luck.
[Edited on 12-6-2011 by AJKOER]
|
|
|
LanthanumK
Hazard to Others
 
Posts: 298
Registered: 20-5-2011
Location: New Jersey
Member Is Offline
Mood: No Mood
|
|
If the protective coating is disrupted, won't the aluminium foil start reacting vigorously with the acetic acid?
hibernating...
|
|
|
Texium
|
Thread Moved 19-11-2023 at 16:36 |
pesco
Hazard to Self

Posts: 95
Registered: 19-11-2015
Member Is Offline
Mood: No Mood
|
|
Electrolysis of sulphate produces solid Zinc. A bit spongy if high current is used.
If you need powder that it would have to be ground what is unnecessary additional work.
Best way to make zinc powder is to electrolyse Na2Zn(OH)4 which is easily made by dissolving ZnO in NaOH.
Dissolving metallic zinc powder might work with a boiling in NaOH.
Electrolysing sodium zincate produces very nice, small grain, metallic zinc powder that is easy to wash and dry.
|
|
|