[*] posted on 27-1-2009 at 16:40
synthetic corundum


I bought an old 1970's METCO metallizing gun secondhand and starting mixing up my own powder mixes and trying them out. I've made some neat gemstone coatings with aluminum powder. I have a book called Gemstones Made by Man(Nassau) that describes Verneuil's flame fusion torch. I've tried to make a fused boule like his process, but can only make small crystals. I'm using oxy-acetylene and his torch used oxy-hydrogen. I wonder if the hydrogen makes a difference? I've noticed that copper powder makes the flame smoke and make lampblack, even when the flame is oxidizing. Why is this? Does anyone have experience with this?
View user's profile View All Posts By User
DJF90
International Hazard
*****




Posts: 2266
Registered: 15-12-2007
Location: At the bench
Member Is Offline

Mood: No Mood

[*] posted on 27-1-2009 at 16:52


I dont think you are making lampblack, but rather copper (II) oxide, which is a black powder. It could form from oxidation of the copper metal in the oxidising flame. I dont think the oxy-fuel system matters, as an acetylene torch can reach ~2700C IIRC, which should be more than enough (possibly more than an oxy-hydrogen torch, I dont know). Try heating a smaller amount of material, as you might not be supplying enough energy with a larger amount.
View user's profile View All Posts By User
Xenoid
National Hazard
****




Posts: 776
Registered: 14-6-2007
Location: Springs Junction, New Zealand
Member Is Offline

Mood: Comfortably Numb

[*] posted on 27-1-2009 at 21:13


Congratulations bluemike, I've often thought of trying this myself.

Are you using aluminium powder or alumina (Al2O3) powder. The Verneuil process calls for alumina powder sprinkled into the flame. The small melted particles are allowed to build up on an alumina rod to form to form the boule. Alumina melts at 2050 oC. One advantage of the oxy-hydrogen flame besides being slightly hotter (2800 oC) would be the lack of contaminants. You may be getting carbides forming which disrupt the corundum crystal lattice.
View user's profile View All Posts By User
not_important
International Hazard
*****




Posts: 3873
Registered: 21-7-2006
Member Is Offline

Mood: No Mood

[*] posted on 27-1-2009 at 22:16


While reading on the layers and inclusion in corundum made using the Verneuil process, I came across a statement that the bubbles were a result of the top layer of the boule actually boiling and capturing small amounts of gas as a result.

As the bp of Al2O3 is just about at the limit of the oxyhydrogen flame, this suggests that the top of the boule and falling drops are really hot, perhaps so fluid that the drops are very fluid and quickly spread out into thin films - the layers seen in the boule. Further assumption is that this spreading widens the boule from the tiny starting bit to the larger boule diameter.
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 28-1-2009 at 04:31


Fascinating subject, though I must admit, at first glance, I thought corundum in the title was a miss-spelling of conundrum.
Correct me if I'm wrong, but isn't ruby simply corundum coloured by chromium.

This gives me one more reason to buy an oxyacetylene torch.

I think, btw, that the oxyacetylene flame is hotter than oxyhydrogen and was one reason oxyacetylene became ubiquitous for cutting and welding.
Now, where are my reading glasses. . .

Homemade emery-paper, bluemike???
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 28-1-2009 at 05:08


Quote:
Originally posted by Xenoid
You may be getting carbides forming which disrupt the corundum crystal lattice.


Good point, Xenoid, CO2 may be unstable above 2000*C, which might make C2H2 a poor choice in this instance.
Back to the DB. . .
View user's profile View All Posts By User
Fleaker
International Hazard
*****




Posts: 1254
Registered: 19-6-2005
Member Is Offline

Mood: nucleophilic

[*] posted on 28-1-2009 at 05:43


Oxy-acetylene is indeed hotter than oxy-hydrogen. Nice thing about O2/H2 is that it's a very clean flame. I always wanted to try the Verneuil process.

Please post up some pictures of the boules you make and your setup.




Neither flask nor beaker.


"Kid, you don't even know just what you don't know. "
--The Dark Lord Sauron
View user's profile View All Posts By User
PHILOU Zrealone
International Hazard
*****




Posts: 2894
Registered: 20-5-2002
Location: Brussel
Member Is Offline

Mood: Bis-diazo-dinitro-hydroquinonic

[*] posted on 29-1-2009 at 08:02


Here is the little a know about the problem...

I rememeber a TV document (a few 14 years ago) that explained that an american society was specialised into the making of synthetic corundum...Their stones where pure and in cristaline shapes, bubbleless, usefull for optical lenses and devices, ranking over the 1 cm diameter...loked like a candy store :D ; but the process was electrothermic and with the help of a secret fundant salt mix (certainly an eutectic that allowed lower mp of the Al2O3)...Synthetical stones so produced were purer than the natural occuring stones and so they dopped their stones with a specific element that provided orange fluorescence, to distinguish the synthetic stones from the natural ones...price was attractive though since it was 1/20th of the price of the natural product!

This gave me the idea to try the making of corundum...
I also have a tiny butane-N2O torch, and a larger Butane-O2 torch with what I was able to make some red ruby pellets (1mm diameter) from Al2O3 white powder and a little green Cr2O3. But with a torch the amount of powder sprayed arround by the gases is big...The container was heat resistant clay in a cup fashion so that the pellets fall back into the melt.

-Al2O3 gives leuko corundum (colourless stone)
-With a little Fe2O3 gives yellow corundum
-With a little Cr2O3 gives the red corundum (ruby)
-With a litlle TiO2 or FeO gives a pale blue corundum
-With a little CoO gives a deep blue corundum (saphire)
So with red-blue-yellow and colourless, one can make a rainbow of corundum...

One might think to use instead of the electricfurnace a sunlight laser (2000-4500°C) furnace to get bubbleless stones...

I hope this helped




PH Z (PHILOU Zrealone)

"Physic is all what never works; Chemistry is all what stinks and explodes!"-"Life that deadly disease, sexually transmitted."(W.Allen)
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 2-2-2009 at 12:43


I believe synthetic sapphire is made by fusing Al2O3 in a molybdenum crucible (inert atmosphere, induction heated) and drawing a boule through a mask if noncylindrical shapes are desired.

Synthetic sapphire isn't too hard to come by; they use it for scratch resistance in supermarket checkout scanner windows. Each pane is probably a few hundred bucks, which considering the size and nature of it, is an excellent deal.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
Saerynide
National Hazard
****




Posts: 954
Registered: 17-11-2003
Location: The Void
Member Is Offline

Mood: Ionic

[*] posted on 2-2-2009 at 20:34


Do post pics if you manage to make the boules! It would be awesome if you faceted them :D



"Microsoft reserves the right at all times to monitor communications on the Service and disclose any information Microsoft deems necessary to... satisfy any applicable law, regulation or legal process"
View user's profile View All Posts By User
chief
National Hazard
****




Posts: 630
Registered: 19-7-2007
Member Is Offline

Mood: No Mood

[*] posted on 2-2-2009 at 23:14


There are several different ways of growing corundum:
==> the Verneul: Rinsing Al2O3-powder down through a downwards-directed H + O-flame
==> the Czochralski: Melting everything, putting a seed in, and pulling that seed slowly out, maybe 1 mm/hour
hight temperature required for the above ways ... ; both give long rods, suitable for laser-applications etc.; but not good for gemstones, because the dopants don't get distributed evenly

There are 2 chepaer ways too, also bettter for gem-quality; I recently saw a website about that, let me see, if I can find it ...
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 3-2-2009 at 07:28


Er, dopants get distributed quite evenly. Rubies? Pffbt, imprecise alchemy, Cr2O3 to 1%. Large silicon boules are regularly grown with parts per trillion doping levels with the Czochralski process.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
Sedit
International Hazard
*****




Posts: 1939
Registered: 23-11-2008
Member Is Offline

Mood: Manic Expressive

[*] posted on 4-2-2009 at 20:05


Quote:
because the dopants don't get distributed evenly


Are you shore about this? The whole principle that a laser basis it self off of requires that the crystal structure and ESSPECIALY the dopant be in as precise manner as possible.
View user's profile View All Posts By User
chief
National Hazard
****




Posts: 630
Registered: 19-7-2007
Member Is Offline

Mood: No Mood

[*] posted on 4-2-2009 at 23:49


The dopants _dont_ get distributed evenly with the verneul, and neither with the czochralski ; no gem-quality possible, but good enough for lasers. The rods, viewed from the side, always have zonar coloring, paler sections and fuller ones.

Of course a world-champion-crystal-grower might succeed in making this quite invisible, but that takes quite some control at the temperatures of 2100 Celsius ....

It's also the same for the dopants in Si-crystals: This was always a problem, until only several years ago, when it was introduced to electromagnetically stir the liquid zone .

[Edited on 4-2-2009 by chief]
View user's profile View All Posts By User
zed
International Hazard
*****




Posts: 2321
Registered: 6-9-2008
Location: Great State of Jefferson, City of Portland
Member Is Offline

Mood: Semi-repentant Sith Lord

[*] posted on 19-5-2009 at 16:40


In natural gemstones, growth lines are "geometrical" and parallel to natural crystal faces. These naturally occurring crystals are generally inferior in superficial appearance, and very few natural stones equal the color and clarity available via the Verneuil or Czochralski processes.

It isn't the presence of growth lines that indicates a gemstone is of artificial origin. More often it is the geometry of those lines. In the simplest cases, these can be easily observed through a jeweler's "eye piece". The Verneuil process produces beautiful gems, that have obviously "Curved" growth lines.

Such crystal growth does not occur in nature.

Of course, most artificial "Colored" stones can be readily identified without even an eyepiece.

They look too good!



View user's profile View All Posts By User
MessyScience
Harmless
*




Posts: 1
Registered: 17-10-2015
Member Is Offline

Mood: No Mood

[*] posted on 17-10-2015 at 19:00


I'm by no means an expert on the subject, but I am fairly sure that crystals (rubies, emeralds, etc.) that are produced through both flame fusion (Verneuil) and the Czochralski are gem-quality. They have both been used extensively in "budget" jewelry. One example off of the top of my head is Stauer. I honestly don't know much about how the dopants are distributed, but apparently they do turn out gem-quality.

So far, it sounds like an oxyhydrogen flame would be needed to avoid carbides and other contaminates.The process traditionally takes place over the course of multiple hours. I know that there are oxygen tanks available but, in terms of practicality, how would one be able to obtain a supply of hydrogen large enough to form a flame four several hours?

I guess that your options would essentially be limited to some sort of metal hydride storage, or to a reaction that produced a steady supply of hydrogen. Electrolysis could be an option.

Any thoughts and other contributions would be welcome. I realize that this is a very old thread, but I hoped that I would be able to find some information and ideas from those more knowledgable than I. Thanks!
View user's profile View All Posts By User
PHILOU Zrealone
International Hazard
*****




Posts: 2894
Registered: 20-5-2002
Location: Brussel
Member Is Offline

Mood: Bis-diazo-dinitro-hydroquinonic

[*] posted on 22-10-2015 at 10:06


Yes Verneuil corundums (ruby and saphire are corundums) are good for optical and for jewelry.
I bought some pears and cylinder for cheap at a mineral fair/salon and even some facetted gemstones... all Verneuil's

In the picture here under:
-50€ for the big cylinder (it is glassy on that side, but very transparent through the section) color from ruby red to violet
-6€ for the orange half pear
-5€ for the pink half pear
-2-3€ for each facetted rubies
Nat-1.JPG - 219kB


In the following picture:
(-green dioptase from Katanga)
(-pale blue quartz gold aqua (quartz bombed with Gold atoms giving a blueish surfacial color (1mm deep penetration))
-27€ for the facetted pale blue saphire
-23€ for the 3 facetted gemstones (deep green & deep blue saphires and the red ruby)
PB220326.JPG - 1.3MB

[Edited on 22-10-2015 by PHILOU Zrealone]




PH Z (PHILOU Zrealone)

"Physic is all what never works; Chemistry is all what stinks and explodes!"-"Life that deadly disease, sexually transmitted."(W.Allen)
View user's profile View All Posts By User
PHILOU Zrealone
International Hazard
*****




Posts: 2894
Registered: 20-5-2002
Location: Brussel
Member Is Offline

Mood: Bis-diazo-dinitro-hydroquinonic

[*] posted on 18-12-2015 at 12:04


Here are my last aquisitions facetted gemstones with Verneuil's process corundums from a mineral fair/salon in Liège (Belgium)..total 115€ very nice quality

In the picture here Under against a AA Battery for scale reference:
-Top 3 violet corundums/saphires
-2 yellow corundums/saphires embaced by two colourless saphires and on the extremes 2 pink rubies (red saphires)
-Below 7 blue corundums/saphires

PC040029.JPG - 1.6MB

I also bought two lasers (one red and one UV).
Interesting feature of red, pink and blue saphires are their bright red-pink fluorescence in the dark when exposed to UV laser/light...
I'll try to make a picture of that fascinating effect. Yeah back into the 80's fluo flash fun :D


[Edited on 18-12-2015 by PHILOU Zrealone]




PH Z (PHILOU Zrealone)

"Physic is all what never works; Chemistry is all what stinks and explodes!"-"Life that deadly disease, sexually transmitted."(W.Allen)
View user's profile View All Posts By User
Texium
Administrator
Thread Moved
22-11-2023 at 19:57

  Go To Top