Conductive Sodium Silicate?


I've been attempting to make a stainless retort for making K, Rb, and Cs metals. Instead of using a tube furnace, I wanted to wind some Nichrome wire around the pipe itself. I first slathered a layer of sodium silicate furnace cement on the pipe and baked it, to electrically insulate the Nichrome from the stainless pipe. After winding the heating element, I added another layer of furnace cement to protect the wire.

During testing, I noticed that once it reached maybe 400C, the wattage would start to climb. I could turn down the variac to correct the wattage, but it would still keep climbing. Eventually I'd see a dramatic power spike, and the element would quickly burn out. I re-built and tested this thing 3 times, with the same results. The highest temperature I measured was about 650C.

So this all leads to my question: Is it possible the sodium silicate cement is becoming conductive at a high enough temperature, and shorting out the coils? This seems strange, but I honestly can't think of any other explanation.
View user's profile View All Posts By User
Morgan
International Hazard
*****




Posts: 1753
Registered: 28-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 21-9-2021 at 13:05


There was this pdf article/title that maybe has something. Soda lime glass isn't very good for high voltage, borosilicate better and pure quartz a good insulator. So maybe the sodium ion is "freeing up" even for your relatively low voltage and high heat. Seems like you have a very thin layer of brittle silicate and the expansion of heated steel if the COE doesn't match, maybe along with the sodium, could be creating a pathway?
But I'm only guessing.

Selected properties of sodium silicate glasses and their structural significance - CORE
"The electrical resistivities of sodium silicate glasses ranging from 7.9 to 40.0 mole % Na20 were determined at 50 hz. and tempera tures fraa 360 to 480*C by Haven and Verkerk"
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5142
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 21-9-2021 at 13:54


Hot glass is a fairly good conductor.
https://www.youtube.com/watch?v=xwEQZw3KPWg
View user's profile View All Posts By User
Metallophile
Hazard to Self
**




Posts: 93
Registered: 23-3-2018
Member Is Offline

Mood: No Mood

[*] posted on 21-9-2021 at 15:03


Thank you both! That pretty much confirms it then. I'll need to find a different cement, or change the design.
View user's profile View All Posts By User
Morgan
International Hazard
*****




Posts: 1753
Registered: 28-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 21-9-2021 at 19:46


It's interesting unlike metals, glass becomes more conductive the hotter it gets. There was this article too using a lightbulb that lights when heated glass starts to slump.

"Insulating glass becomes a conductor of electricity when heated red-hot with a blowtorch."
https://sciencedemonstrations.fas.harvard.edu/presentations/...
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1800
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 22-9-2021 at 07:16


I did something quite similar using sodium silicate and talcum, it lasted for years at temps up to 900°C. This came from an old CRC handbook claiming it could handle temperatures up to 1000°C.



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
macckone
Dispenser of practical lab wisdom
*****




Posts: 2214
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 22-9-2021 at 08:41


Sodium ions are mobilized at high temps in a silica matrix.
This leads to the ability to put a light bulb in salt and produce sodium inside the bulb.
This is a classic experiment: http://www.sciencemadness.org/talk/viewthread.php?tid=148098