Author: Subject: Unexpected flames
Sulaiman
International Hazard
*****




Posts: 3947
Registered: 8-2-2015
Member Is Offline


[*] posted on 3-8-2025 at 21:20
Unexpected flames


I re-melted 16+ kg of lead with all lead waste (dross etc.) that I had,
having read more about lead cleaning/refining since my first attempt
I used candle wax as a flux and a very dry wooden stirring stick.

I think that in my first attempt I used too low a temperature,
so this time I decided to turn the heat to max.

Here is what happens when the lead exceeds the autoignition temperature of candle wax :)

https://youtube.com/shorts/qQpYCdDTtIw?si=z9SKtxVvc3ZG9YXz




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5142
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 4-8-2025 at 01:03


Ignition temperatures depend on the surface.
It's also possible that the flames were ignited by a hot spot formed when some lead oxide was exothermically reduced by the wax.
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3947
Registered: 8-2-2015
Member Is Offline


[*] posted on 4-8-2025 at 01:20


True, also I used open gas flames for heating,
... I played with it a little,
covering the pot extinguised the flames
but when the cover was removed the pot burst into flames again within seconds..
(could be wax vapours reaching the flames below?)
Anyway, my main point of posting is to warn and possibly amuse some members,
because the videos that I've watched , where wax was used as a flux for lead
never showed spontaneous combustion.




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
teodor
International Hazard
*****




Posts: 1169
Registered: 28-6-2019
Location: Netherlands
Member Is Offline


[*] posted on 4-8-2025 at 02:29


I didn't know you need a flux for lead. But if you really need to protect the top layer from oxidation you can try to find some soluble salt of a relatively weak acid with the melting point just above the melting point of lead and that one which is not decomposing. It will form a good protective layer above the liquid lead when molten and you can easily wash it out when cold.
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3947
Registered: 8-2-2015
Member Is Offline


[*] posted on 4-8-2025 at 03:09


I did not want to use borax etc. as I want to keep the antimony in the alloy
(lead scrap, old tin:lead solder and battery plates)

The lead has now cooled, this is how it came out of the pot

top
IMG_20250804_190504.jpg - 4.3MB

bottom
IMG_20250804_190434.jpg - 3.3MB

I think that it is now clean enough to cast.




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1796
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 4-8-2025 at 04:40


Yes, this is common in my experience. I always ignited the fumes anyway to keep the smell down, and to prevent a huge fireball when the smoke inevitably ignites.

@teodor: Lead needs fluxing if you want pure metal. The oxidation rate of molten metal in air is actually fairly slow, so a lid is usually enough to prevent any significant loss. But without fluxing you often get a oatmeal-like mix of metal and oxides that won't cast well. Some claim that the oxide is reduced by the flux, I sincerely doubt it. The boiling point of wax is simply too low for this. I believe it simply breaks the adhesion between metal and oxides.




We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3947
Registered: 8-2-2015
Member Is Offline


[*] posted on 4-8-2025 at 20:00


Quote: Originally posted by Fulmen  
...Some claim that the oxide is reduced by the flux, I sincerely doubt it...
I am inclined to believe that something has reduced most of the oxide that I added back to the pot.
I had lots of dross, but after this run I had quite a lot of charcoal and a surprisingly small amount of dross.
(considering that more than half of the lead was from old diving weights, and quite a lot from corroded battery plates)

I used a dry wood stick because the charring of it releases, amongst other stuff, carbon monoxide - capable of reducing lead oxide.
That is something like what I read anyway.
I guess that the hot vapourised wax, or its combustion products, may also reduce lead oxide.
I am a complete beginner at this, so I accept all advice.




CAUTION : Hobby Chemist, not Professional or even Amateur