Author: Subject: Electroforming Copper Liners
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 11-9-2011 at 14:57


I just tried today to remove the cone actually, and the copper was thin at the base of the cone (close to where the plating solution meets the aluminum form). The short piece of copper pipe was also a bit too loose which caused a problem with removal. By the time I got the cone off I had damaged it quite badly. The aluminum form was also oxidized/eroded quite badly where the form met the surface of the plating solution. Oh well, it had only been plating for two days, no big loss.

I think I may have a solution to the problem though. If just the cone part of the form were exposed and well submerged below the surface of the plating solution, and the submerged sides of the form covered with an insulating material, I believe this would solve both problems. I am trying electrical tape right now. It was carefully wrapped around the forum, leaving just the cone exposed, then well submerged in the plating solution. If the electrical tape does not work, I am sure something else will.
View user's profile View All Posts By User
gnitseretni
Hazard to Others
***




Posts: 290
Registered: 5-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 11-9-2011 at 18:27


Quote: Originally posted by Hennig Brand  
I just tried today to remove the cone actually, and the copper was thin at the base of the cone (close to where the plating solution meets the aluminum form).


That's due to evaporation. The level keeps dropping as water evaporates. The cone will be paper thin at the very top and gradually increase in thickness to wherever the level is at when you stop plating.

Add water to make up for evaporation and keep it at the exact same level it was at when you started plating and you should get a thicker edge that the piece of plumbing pipe will butt up against so you can push the cone off.

Quote: Originally posted by Hennig Brand  
The aluminum form was also oxidized/eroded quite badly where the form met the surface of the plating solution.


Yup, same problems I've been having. That's usually also the only place where the cone is stuck to the form. I use a sharp thin knife and carefully pry it between the cone and the form and go round and round until it pops off. But I like your idea of using a "puller" better.

Quote: Originally posted by Hennig Brand  
I think I may have a solution to the problem though. If just the cone part of the form were exposed and well submerged below the surface of the plating solution, and the submerged sides of the form covered with an insulating material, I believe this would solve both problems. I am trying electrical tape right now. It was carefully wrapped around the forum, leaving just the cone exposed, then well submerged in the plating solution. If the electrical tape does not work, I am sure something else will.


Let us know how it works out. I've tried Sharpie myself.. didn't work. (Worth a try :P ) I thought about using tape but thought the plating solution would probably find a way to get in between the tape and the form. If the tape doesn't work, maybe a layer of paint or varnish or something.
View user's profile View All Posts By User
Mr. Wizard
International Hazard
*****




Posts: 1042
Registered: 30-3-2003
Member Is Offline

Mood: No Mood

[*] posted on 12-9-2011 at 09:02


Regarding the corrosion on the aluminum forms, be aware they might be using an alloy of zinc and aluminum for these. There is a spectrum of purity in 'white metal' alloys which are heavily recycled. Even aluminum beverage cans have a mixture of products. As the purity goes down, this admix of copper, lead, tin, zinc, magnesium, and everything that will melt gets used to form this non demanding product.
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 12-9-2011 at 13:31


With all the aluminum products out there, I guess one would need to be careful that they were getting the right thing. I think that most round stock from a machine shop would have a very definite composition though. Admittedly, I forgot to ask what the composition of the aluminum round stock I purchased was.


Here is a basic description of my method for turning aluminum cones.

It is not very difficult to make a cone on a lathe. Just make sure the round stock is chucked as straight as possible, after that you can't really go wrong. As long as it is well centered in the chuck and is going around in a perfect circle, you are almost guaranteed a perfect cone shape. At the very end just take small cuts so as not to leave excessive roughness. Finally use emery cloth, progressively using finer and finer emery cloth until the form is as smooth as glass.

For making smaller forms on the lathe you can easily just use a metal file instead of a cutter, and then emery cloth. I guess you could use a file for the big cones too, but it would take much longer.


[Edited on 13-9-2011 by Hennig Brand]
View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2011 at 09:06


Quote: Originally posted by Hennig Brand  
With all the aluminum products out there, I guess one would need to be careful that they were getting the right thing. I think that most round stock from a machine shop would have a very definite composition though. Admittedly, I forgot to ask what the composition of the aluminum round stock I purchased was.
Most aluminum alloys in machine shops are alloyed with something: silicon, magnesium, zinc, etc. There are lots of them. The 1xxx series of aluminum alloys are all minimum 99% Al content. Alloy 1199 is 99.99% pure aluminum.
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2011 at 15:51


Thanks for the information. I remember seeing some lettering along the length of the round stock but I didn' t have a lot of choice at the time anyway (I took what they had). It sounds like what I have is probably fine.

I left the 3/4" aluminum form to plate for 3 days. This time the cone popped off very easily with a little pressure from the puller. I had to get a sleeve for the puller that fit the aluminum form better. With some help a piece of an old lamp stand was cut out to a perfect fit. Using the tape as a stop-off to shield the part of the form where plating wasn't desired and to prevent form corrosion was a big success. This is great because it is so easy to wrap a little electrical tape on before plating and remove it after plating is complete.

I have found that it is best to plate with very low current. Slower plating with low current produces smoother and more even plating. My plating bath was run for 3 days at about 50mA. My cone is only 3/4" diameter. If the cone is larger, or the surface area to be plated is larger, the plating bath will require a proportionately larger current to provide the same current density.

Anyway, here are some pictures. I am starting to get some decent results. The bottom of the cone was left a little rough for now. I may do a little more sanding later. Note that the oxidation seen on the aluminum form, in the second picture, was from the previous run without the tape.

Fresh from bath.JPG - 178kB Tape off.JPG - 176kB In puller.JPG - 175kB Cone off.JPG - 190kB Pieces.JPG - 195kB Cone (3 quarter inch).JPG - 173kB Cone.JPG - 192kB


[Edited on 15-9-2011 by Hennig Brand]
View user's profile View All Posts By User
gnitseretni
Hazard to Others
***




Posts: 290
Registered: 5-1-2007
Member Is Offline

Mood: No Mood

[*] posted on 14-9-2011 at 16:31


Nice cone! Can't wait to see how it performed ;)
Good to know the tape was a success.
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 15-9-2011 at 07:41


Thanks, this is a good pastime. Once everything is setup, it is about as difficult to look after as a goldfish.

This is sort of interesting. It is a lab manual designed to help teachers run a lab on copper plating, or do a lab demontration on copper plating. It is a good introduction to the subject I would say.

Attachment: THE CHEMISTRY OF COPPER PLATING.pdf (192kB)
This file has been downloaded 3380 times


[Edited on 15-9-2011 by Hennig Brand]
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 20-9-2011 at 12:48


The copy/paste below is from the following link. The whole web page is worth a read. Actually the entire web site looks quite interesting.

http://www.dalmar.net/electroforming.htm

"Trouble shooting electroforming

Two of the biggest mistakes made in Electroforming are

(1) not getting a good connection from the lead wire to the work piece. If you are making a piece of jewelry, you should glue a finding on the piece before you start. When applying the conductive coating, make sure that you cover the glue and part of the finding to make sure that you have a good connection. If you have a work piece that is not jewelry, you should take a piece of copper wire
and bend about 1/4 inch of the wire at the end to a 45 degree angle. Glue
this end of the wire to the work piece in an inconspicuous place like the back
of the piece. Again make sure when applying the conductive coating that you
cover the end of the wire and glue to get a good connection. After you have
finished the copper stage you can clip off the wire and file it smooth. For
your next finish over the copper you can just wrap the wire around the
piece. Don't wrap the wire around the piece when you are electroforming in
copper. If you do this, more than likely you will get a bad connection and the
wire will become part of the work piece due to the thickness that you are
growing. A sure sign of a bad connection between the wire and the
work piece is the crystallizing of the copper on the copper wire with
no growth on the work piece.

(2) The biggest mistake made in electroforming is not setting the machine
to the proper amperage for the area that you are electroforming in the tank
or using a rectifier that is too powerful and won't adjust to the proper
setting. 90% of the technical calls to our company about electroforming are
due to this mistake. You must set the rectifier to 1/10 of an amp per square
inch of metal surface that you are electroforming in your tank with the
copper solution. If your setting is too low the copper will build-up with
a shrimp color on it. If the setting is right it will come out like a new
penny. If the setting is too high you will get a dark color and a
bumpy finish that looks like fried chicken. Also make sure that the size
of your anodes is equal or greater then the total of surface that you are
electroforming in the tank."

I included a picture with basic formulae for cones. The surface area formula would be useful when trying to determine the proper electrical current to use when electroforming.

Area of cone.jpg - 14kB
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 3-6-2012 at 16:01
Copper Electroforming & Troubleshooting


This is the best write-up I have seen so far. The whole thing is worth a read, but it also has quick reference tables with lots of good information. About half way through there is an acid copper troubleshooting guide which is particularly useful.

Attachment: Copper_Plating.pdf (187kB)
This file has been downloaded 2786 times



[Edited on 4-6-2012 by Hennig Brand]




"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
SjeefOne
Harmless
*




Posts: 2
Registered: 21-7-2010
Member Is Offline

Mood: No Mood

[*] posted on 4-6-2012 at 00:07


Thnx for the doc, looks like a valuable read!

I've been starting some electroforming experimenting as well recently and thought I'd share some of it.

The pdf from gnitseretni is what I kind of used as a guide as of how to set my cell up.

For my anode I've used copper brake line bent into a coil shape, my former is turned from aluminum, this particular one is 24mm with a cone angle of 60 degrees.
The electrolyte is a solution of about 150g of CuSO4 and 25ml of H2SO4.

Cell.jpg - 53kB

I found that it is indeed important to keep the voltage low, at high(er) voltage the copper will form way to quick and becomes a brittle layer which is easily wiped off.

At low voltage (below cone was formed at around 2V and .5Amps) the layer builds quite nice and dense. However i'm now facing problems getting the cone of the former. I'm therefore am having some new formers made and a puller as well, which I hope will help get the cones off :)

Cone.jpg - 41kB
My first cone.
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 4-6-2012 at 06:49


You could check the coefficients of expansion of both metals.
If copper has the higher rate, heating the cone with a heatgun might shift it ─ if aluminium has the higher rate, cooling it in a freezing mixture might work . . .

View user's profile View All Posts By User
SjeefOne
Harmless
*




Posts: 2
Registered: 21-7-2010
Member Is Offline

Mood: No Mood

[*] posted on 4-6-2012 at 07:24


Looks like Al has a higher coeficient then Cu..
I'll put my former in the freezer see if anything gives.

View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 6-6-2012 at 16:53


I just recently got back into electroforming and things have not gone perfectly smoothly. I realized after about a week of messing around that I had gotten soldering flux into my plating bath which caused a lot of problems with the plating process. Copper was "burning" easily, even with low current and would not plate in a smooth layer. I started over with fresh electrolyte, but a little flux must have been on the anodes still. The resultant cone is the one in the pictures. It electroformed much better, but not perfectly smoothly and needed to be filed and sanded down on the lathe.
I thought I was doing a good thing by soldering the connections on my electrodes, but I actually ended up poisoning my plating bath. The flux should have been carefully cleaned off after soldering, or soldering should not have been done at all.

I have also had problems with the older lathe that I have been using. It is not very precise anymore and has been making aluminum cone forms that are not entirely symmetrical.

At the same time the electrolyte was changed, the sulfuric acid was changed from drain cleaner to battery electrolyte. There are a lot of impurities in drain cleaner, and it is not always the same impurities from brand to brand and from lot to lot. I figured that battery electrolyte would need to be fairly pure to function properly in a battery.

An aquarium air pump and bubbler were used for agitation. This was a bit messy, but manageable. Electrical tape was used as a stop-off to prevent the aluminum form from being oxidized which worked very well. Careful application of the tape also controlled exactly where the form was plated, and allowed the area on the form being plated to be submerged well below the surface of the plating bath.

I have found that a current density between 0.06A and 0.08A per square inch is optimal for my setup, any more results in burned copper. Without brighteners and other additives the goal should be to achieve a smooth, even coat of salmon colored copper. Without brighteners salmon colored copper is normal right out of the bath. The copper can later be polished to a new penny look after plating.

The power supply in the picture is a switching supply which was taken out of a large photocopier about 10 years ago. The box with the dial on it has a large bank of huge 200-300 watt power resistors in it. It goes from 0 to 33 ohms in increments as the dial is turned. In order to get resistance values between increments an external resistor must be used. The white ceramic inline resistor in the picture is rated for 5 W & 2 ohms. Measuring the voltage drop across this resistor is a quick way of determining the current flow through the plating bath without interfering with its operation (I = V/R).

A much overbuilt puller was made which removed the cone with ease after sanding and polishing was completed on the lathe.

BTW, the cone in the pictures is 1.5 inches in diameter.


Cone 1.JPG - 306kB Cone 2.JPG - 634kB Cone 3.JPG - 340kB

Cone 4.JPG - 274kB Cone 5.JPG - 297kB Cone 6.JPG - 201kB

Cone 7.JPG - 346kB Cone 8.JPG - 214kB Cone 9.JPG - 242kB

[Edited on 7-6-2012 by Hennig Brand]




"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
froot
Hazard to Others
***




Posts: 347
Registered: 23-10-2003
Location: South Africa
Member Is Offline

Mood: refluxed

[*] posted on 6-6-2012 at 23:00


A chap I met recently used to make these for the millitiary. His formers were parabolic shaped 'trumpet' like cones made from stainless steel and pretty much the same size as the ones you guys are making here. The copper liners he electroformed were about 0.5 mm thick and uniform all over.
I would imagine that stainless steel does not passivate like aluminium does ensuring good initial plating performance is less chance of it contaminating the bath. A good source of stainless would be in the form of stainless steel bolts from the local hardware which you could turn into cone formers.




We salute the improvement of the human genome by honoring those who remove themselves from it.
Of necessity, this honor is generally bestowed posthumously. - www.darwinawards.com
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 8-6-2012 at 15:05


I have wanted to try stainless steel for a while. I actually purchased some 1 inch SS round stock about a week ago, but then I stuck with the aluminum forms for the time being. The nice thing about aluminum is that it is so much easier to work. I am going to have to try stainless though, it may be worth the extra effort.



"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
NeonPulse
Hazard to Others
***




Posts: 417
Registered: 29-6-2013
Location: The other end of the internet.
Member Is Offline

Mood: Isolated from Reality! For Real this time....

[*] posted on 6-2-2014 at 20:20


Quote: Originally posted by gnitseretni  
I managed to electroform two copper liners. I did a quick writeup on it (with lots of pics) that shows how I made them. Thought I'd share it in case others would like to try it ;)


what a great idea! i have one in the plating bath right now. i got the form from ebay a nice Al fence cap that was slightly flat at the tip but there was excess n the tip so i could file it to a point. i followed gnitseretni's PDF with an alteration to the anode and slightly stronger power supply. and it is working a treat. great idea! your process has certainly won me over! cant wait to test its performance though. i expect it it to work very well.;)




Where there is a will
there is a way.

AllCheMystery!
https://www.youtube.com/channel/UCWbbidIY4v57uczsl0Fgv7w?vie...
View user's profile View All Posts By User
froot
Hazard to Others
***




Posts: 347
Registered: 23-10-2003
Location: South Africa
Member Is Offline

Mood: refluxed

[*] posted on 6-2-2014 at 22:26


I know this is a little late but to ensure uniform density and thickness of the liner you should rotate the cathode slowly in the solution. Additives called 'brighteners' are used to give a smooth shiny plate which indicates a good high density high strength form. I would expect any porosity to negatively affect the performance of the liner.



We salute the improvement of the human genome by honoring those who remove themselves from it.
Of necessity, this honor is generally bestowed posthumously. - www.darwinawards.com
View user's profile View All Posts By User
packetforger
Harmless
*




Posts: 48
Registered: 21-2-2014
Member Is Offline

Mood: Condensing

[*] posted on 21-2-2014 at 05:48


Has anyone checked if the purity of copper metal used affects the finished product? I would imagine having the copper (anode?) made of pure copper foil, and "around" the anode (as in, cylindrical anode, with the cathode in the center of it) would help with giving excellent results.

As would using high quality coppersalt and acid without nasty gunk contaminants (boiling drain-cleaner grade sulphuric wiith activated charcoal, followed by filtration through glass wool works good to decolourize it of organic? contaminants).

I will have to aquire some barstock and try this out, am very curious about the mechanical properties of the formed copper piece. Could be interesting for making small conductiveparts for RF stuff!
View user's profile Visit user's homepage View All Posts By User
Vlad1111
Harmless
*




Posts: 2
Registered: 11-10-2014
Member Is Offline

Mood: No Mood

[*] posted on 12-10-2014 at 05:56


Hi

I`ve read really much about copper plating but even after several tries, the results aren`t that good

At the moment i try to copperplate a plastic cone* (3 layers of L100 conducting silver) this a 4.8V-400mA chellphone charger.
Standoff between the anode and cathode is around 1cm (~1/3 inch) at around 16°Celsius (60.8°F)

*radius ~3cm (~1inch) hight is around 5.8cm (~2,2inch)

The process is working for one day now and ive seen that the surface of the plated cone is extremely rough.
most of the cone is a extremely thin layer. the surface is exactly like sandpaper:(

i tried to plate under the exact conditions an smaler cone* (stainless steel [without L100] and the surface was so smooth you could barely see it was plated in the plating solution)

*radius ~1.5cm (~1/2inch) hight is around 4cm (~1 1/3inch)

Plating solution: 500ml water - 100g CuSO4.6H2O - 25ml H2SO4 - no NaCl

so, can anyone tell me what am i doing wrong?
im getting desperate:mad:
View user's profile View All Posts By User
Oscilllator
National Hazard
****




Posts: 659
Registered: 8-10-2012
Location: The aqueous layer
Member Is Offline

Mood: No Mood

[*] posted on 20-10-2014 at 16:27


Quote: Originally posted by Vlad1111  
Hi
I`ve read really much about copper plating but even after several tries, the results aren`t that good

At the moment i try to copperplate a plastic cone* (3 layers of L100 conducting silver) this a 4.8V-400mA chellphone charger.


Quote: Originally posted by SjeefOne  

I found that it is indeed important to keep the voltage low, at high(er) voltage the copper will form way to quick and becomes a brittle layer which is easily wiped off.

At low voltage (below cone was formed at around 2V and .5Amps) the layer builds quite nice and dense.

Please take 30 seconds to read the thread before posting. It isn't that hard.
View user's profile View All Posts By User
dangerous amateur
Hazard to Others
***




Posts: 150
Registered: 8-7-2011
Member Is Offline

Mood: No Mood

[*] posted on 25-2-2015 at 08:28


Do you guys think it is necessary to agitate the solution?

And how about the target being placed slightly asymmetric to the anode, will this cause the plating to become uneven?


It seems to me that the electrolyte is so conductive that it does not matter, but I would like some other opinion on that.
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1796
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 25-2-2015 at 09:03


Current density will affect deposit rates.



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
Camroc37
Hazard to Others
***




Posts: 101
Registered: 4-8-2015
Location: USA
Member Is Offline

Mood: Must...Nitrate...EVERYTHING!

[*] posted on 25-4-2016 at 18:55


Quote: Originally posted by Hennig Brand  
I originally posted this in the unconventional shaped charge thread. It was suggested to me that this was a more suitable place to post it, so here it is(...)


Could you explain a bit more about this setup? Is the Cathode running from the top right in the picture and the anode under the cone? Thanks.


[Edited on 11-9-2011 by Hennig Brand]




Youtube channel is Camroc37.
I make chemistry videos.
https://www.youtube.com/channel/UCpvdD2LIyXA34jvhPlUXorQ
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
View user's profile View All Posts By User
XeonTheMGPony
International Hazard
*****




Posts: 1641
Registered: 5-1-2016
Member Is Offline

Mood: No Mood

[*] posted on 29-4-2016 at 07:46


I have don tones of copper plating, I once copper plated cardboard! Why? Because I thought it would be funny! (It was!)

Trick, gently circulate your tank solution, makes for a very even coat, current control is every thing So is voltage, if you can't control both you can end up with a head ache! Use an all copper tank, do what you have too but the better the tank is clad the better the plate.

I used a bubble to keep the solution moving during plating.

Graphite is a great starter! for the paper plating I started off very slow to get a thin even copper coat then I drove the voltages up slowly to get the proper current flow Vs surface area.

To coat the paper I made a graphite paste and worked it in to the surface and a bit of glue to help hold the paper together in the bath.

I would wager one can modify my method by making a pulp slurry with graphite mixed in, mold the cone, then smooth the out side and spray lacquer on the inside to insulate it, this should make a readily dissoluble mold.