Author: Subject: Cracks disappearing
Nickbb
Harmless
*




Posts: 25
Registered: 6-12-2012
Location: 3rd dimension
Member Is Offline

Mood: something other than a chemistry pun

[*] posted on 25-12-2012 at 19:12
Cracks disappearing


I recently posted a topic on how to fix a retort I had and before I could fix it, I had gotten it out and lo and behold the crack wasn't there! Is it possible for glass to just fuse back together by itself? I've never seen that before.
View user's profile View All Posts By User
Oscilllator
National Hazard
****




Posts: 659
Registered: 8-10-2012
Location: The aqueous layer
Member Is Offline

Mood: No Mood

[*] posted on 25-12-2012 at 19:23


I have done it, mind you it wasn't at room temp though. My one and only test tube had a crack in the bottom so I whipped out my propane lamp and heated it to softening point. The crack literally disappeared before my eyes, although once it had cooled down there was still a faint trace of were it had been before.

I dont think it can fuse together by itself, though.




View user's profile View All Posts By User
zed
International Hazard
*****




Posts: 2319
Registered: 6-9-2008
Location: Great State of Jefferson, City of Portland
Member Is Offline

Mood: Semi-repentant Sith Lord

[*] posted on 3-1-2013 at 18:19


No longer visible, is not the same as non-existent. You can't see the crack right now.

Unless it has been hundreds of years since you last used the glasswear, it is unlikely that it has healed itself.
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 4-1-2013 at 02:06


I think glass flows slower even than that . . .
View user's profile View All Posts By User
Siggebo
Harmless
*




Posts: 23
Registered: 6-5-2012
Location: Sweden
Member Is Offline

Mood: Under reflux

[*] posted on 4-1-2013 at 04:32


Glass does not flow! This myth needs to be beaten to beyond death...
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 4-1-2013 at 05:13


Glass flows at a slow rate that makes proof of flow impossible to demonstrate . . .
But this doesn't mean glass is not a super-cooled liquid!
View user's profile View All Posts By User
jock88
National Hazard
****




Posts: 505
Registered: 13-12-2012
Member Is Offline

Mood: No Mood

[*] posted on 4-1-2013 at 05:29



Is it not true that old stain-glass windows sag due to flow of the glass.

Ice flows in icebergs. Of course the pressure is large.

Retorts etc, when cracked, do not fix themselves.

I wonder would the stuff that is used to fix cracks in car window screens be used to 'fix' the crack. The stuff is sucked through the crack from one side of the window. I would be very very wary of a retort or any glass ware 'fixed' that way.
View user's profile View All Posts By User
Endimion17
International Hazard
*****




Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline

Mood: speeding through time at the rate of 1 second per second

[*] posted on 4-1-2013 at 05:32


Glass is not a supercooled liquid. It's not that simple. It has crystalized domains. It is an atypical type of matter which we call - glass. :)
Metals can be turn into metallic glasses by rapid cooling, but that doesn't mean they're liquids.

Liquids aren't just characterized by their long range disorder. It's the ability to flow, however small that rate is. Liquids are fluids, and fluids flow. If it doesn't flow, it isn't a fluid, therefore it isn't a liquid.

Glass was never ever proven to flow (unlike extremely viscous organic liquids). Those old chubby church windows - it's a myth. They're chubby upwards or downwards, depending on how they were installed. It's connected to the lousy flattening process which was used long time ago.



@jock88: The liquid used for repairing car windshields just has the same/similar refraction index. They don't repair anything.
Cracks on flasks can be repaired by heating it slightly above its softening range. The pieces join because they're polar and they just exclude air. Sometimes minute air bubbles might remain, but that's a minor problem. What is important is to anneal the glass properly immediately after. Of course, such flask will never have the same strenght, but it can be used for less demanding things.

[Edited on 4-1-2013 by Endimion17]




View user's profile Visit user's homepage View All Posts By User
jock88
National Hazard
****




Posts: 505
Registered: 13-12-2012
Member Is Offline

Mood: No Mood

[*] posted on 4-1-2013 at 05:39



http://www.glassnotes.com/WindowPanes.html

No flow!
View user's profile View All Posts By User
sargent1015
Hazard to Others
***




Posts: 315
Registered: 30-4-2012
Location: WI
Member Is Offline

Mood: Relaxed

[*] posted on 5-1-2013 at 10:18


Hmmm, my distinguished Inorganic Chemistry professor told us that glass flows. I'm going to trust her over a website...



The Home Chemist Book web page and PDF. Help if you want to make Home Chemist history! http://www.bromicacid.com/bookprogress.htm
View user's profile View All Posts By User
Vargouille
Hazard to Others
***




Posts: 380
Registered: 16-4-2012
Member Is Offline

Mood: No Mood

[*] posted on 5-1-2013 at 10:30


Would an ACS article stating that glass doesn't flow be better?

http://pubs.acs.org/doi/abs/10.1021/ed077p846
View user's profile View All Posts By User
Siggebo
Harmless
*




Posts: 23
Registered: 6-5-2012
Location: Sweden
Member Is Offline

Mood: Under reflux

[*] posted on 5-1-2013 at 10:32


Then she needs to be undistinguished at once.

My analytical chemistry professor repeatedly wrote Fl- for fluoride. We winced every single time.
View user's profile View All Posts By User
kavu
Hazard to Others
***




Posts: 207
Registered: 11-9-2011
Location: Scandinavia
Member Is Offline

Mood: To understand is to synthesize

[*] posted on 5-1-2013 at 10:38


Quote: Originally posted by sargent1015  
Hmmm, my distinguished Inorganic Chemistry professor told us that glass flows. I'm going to trust her over a website...

Professors are humans too, they do not posses the ultimate knowledge. Many proffs have said that rather than having exact answers they can only provide rather good estimations based on their academic experience. Moral of the story, don't believe everything they say!
View user's profile View All Posts By User
jock88
National Hazard
****




Posts: 505
Registered: 13-12-2012
Member Is Offline

Mood: No Mood

[*] posted on 5-1-2013 at 14:33


Ask the distinguished professor where she found that out.
View user's profile View All Posts By User
turd
National Hazard
****




Posts: 800
Registered: 5-3-2006
Member Is Offline

Mood: No Mood

[*] posted on 6-1-2013 at 11:17


Quote: Originally posted by Endimion17  
Glass is not a supercooled liquid. It's not that simple. It has crystalized domains. It is an atypical type of matter which we call - glass. :)
And even if it hadn't any crystalline domains it'd still be an amorphous solid and not a slowly flowing fluid.
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 6-1-2013 at 14:27


In principle, a crack could reseat itself -- the molecules are still there, grasping for electrons, happy to get what they can. I think the actual physics of a glass fracture are more complicated than that, though (of course!).

Besides the obvious nanometer scale realignment required for a large contact area, air is exposed to the fresh surfaces, oxidizing some hanging Si bonds; if there's any humidity, water reacts, forming Si-H and Si-OH ends (which won't stick back together), and any adsorbed water will essentially form a lubricating monolayer (or more).

The classical solution to adsorbed substances, hydroxyls and bonding things in general, of course, is fire. And lots of it.

I wonder if any studies have been done on glass fracture in a vacuum. It might be a practicable experiment to take a glass fiber, break it, and mash the ends back together precisely enough to restore it.

But in general, yeah, cracks are always there. By geometry or by lighting condition, you might not be able to see them, but a polarimeter will see the gap and the strain around it.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
Fantasma4500
International Hazard
*****




Posts: 1682
Registered: 12-12-2012
Location: Dysrope (aka europe)
Member Is Offline

Mood: dangerously practical

[*] posted on 8-1-2013 at 09:39


about this.... liquid glass.. im still reading, but im just saying.. i was explained the reason that it flows is because it in between the sheets of apparently SiO2 its still a tiny tiny bit liquid, also as i read abit down (going to read further, still) i think surface tension would play a role in this, the thinner the glass, the less it sinks together, also if you have a window thats really thick, then theres more pressure per cm3 in the bottom than in the top, because of gravity..
if you take 100 metre tall tube of water, the pressure in the bottom will be higher than just 10 cm down from the top..

im definately not denying facts, but by this it could sound reasonable, and also making the exambles used with the very fine glass pieces unusable

just once again so you dont forget, no im not denying what it says.




~25 drops = 1mL @dH2O viscocity - STP
Truth is ever growing - but without context theres barely any such.

https://en.wikipedia.org/wiki/Solubility_table
http://www.trimen.pl/witek/calculators/stezenia.html
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 8-1-2013 at 17:22


As "liquid between sheets" goes, there's a certain grain of truth to that, just not at this temperature. At surprisingly low temperatures, sodium ions do become mobile -- in fact, if you have sensitive enough measurements, I guess they are mobile at room temperature. (That doesn't mean the ions will "drip out" over time, or that the silicon lattice is necessarily weakened -- it can still be rigid, say, like water percolating through concrete.)

I say this because some early semiconductors had problems with sodium ion impurities: indeed, the MOSFET (which today dominates use in almost every chip produced today) was discovered theoretically very early (before 1920 I think), but practical devices wasn't created until the 60s because the process had to be refined, purified and perfected so thoroughly until they were finally marketable.

The biggest problem they had was sodium ions (and something called surface states, also related to impurities), some of which would get trapped in a vital layer of (amorphous -- glass!) silicon dioxide. When a voltage was applied to this layer, turning on the transistor, the electric field would pull sodium ions through it, displacing them and changing the static electric field in the layer. Next time you went to use the transistor, it would turn on at a different voltage! This is like turning on your kitchen faucet and not knowing whether the knob has to be turned 30 degrees or 120 degrees to get a gentle flow rate, and worse, the flow of water causes the threshold to change over time.

(Just to close the story -- modern devices, of course, are made at such extraordinary purity standards that, not only are those threshold voltages highly repeatable within a given device, but a metal terminal, isolated by glass, can be charged at the factory to a particular voltage, and just left there, insulated, a capacitor with no resistance to discharge it, for *decades*, even at elevated temperatures. These have been used as *voltage references* before. On a more crude, digital level, this is what Flash memory does, except with billions of ones and zeros per chip!)

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!