Author: Subject: Easy Colourful Quantum Dots
Housane
Hazard to Others
***




Posts: 127
Registered: 3-9-2018
Location: Worcester, England
Member Is Offline

Mood: Let’s make

[*] posted on 17-6-2020 at 14:17
Easy Colourful Quantum Dots


Today I managed to make green carbon quantum dots by dissolving 3g of sucrose in 10ml of water and 1ml of 30% HCl was added to make it acidic. It was then heated at 80-90C for 10 minutes and the water was allowed to evaporate. After 5 mins the solution turned yellow and it got steadily darker. After the 10 mins a distinctly sweet our could be smelt.

It was take off the heat and allowed to cool. The remaining black solution was dissolved in 150ml of water and then filtered, a dark filtrate was collected. This was made neutral by addition of NaOH. These are quantum dots but to see them clearly i diluted them. In the pictures the range on the lower level is 2 fully concentrated then 5 vials going from 25% to 5% in 5% increments. Feel free to ask any questions. The glow is poor as the light is a cheap UV invisible ink pen, I will do better pictures on request.

Regards

Housane

IMG_20200617_225715.jpg - 396kB IMG_20200617_225736.jpg - 263kB IMG_20200617_225703.jpg - 518kB

[Edited on 18-6-2020 by Housane]




Green QD's so far

Feel free to correct grammar or incorect knknowledge. We are all learning.
View user's profile View All Posts By User
Housane
Hazard to Others
***




Posts: 127
Registered: 3-9-2018
Location: Worcester, England
Member Is Offline

Mood: Let’s make

[*] posted on 17-6-2020 at 14:21
More pictures




IMG_20200617_225748.jpg - 330kB IMG_20200617_225753.jpg - 402kB IMG_20200617_225820.jpg - 2MB




Green QD's so far

Feel free to correct grammar or incorect knknowledge. We are all learning.
View user's profile View All Posts By User
Ubya
International Hazard
*****




Posts: 1247
Registered: 23-11-2017
Location: Rome-Italy
Member Is Offline

Mood: I'm a maddo scientisto!!!

[*] posted on 17-6-2020 at 17:26


i have a request for you, could you check in a few months/a year if they still fluoresce the same?
i made some blue quantum dots via the hydrothermal method (pretty much the same thing you did but in a closed vessel and at 180°C instead of 90) a year and a half ago, and now the solution fluoresces green and it is much much fainter, i suspect that with time the nano particles aggregate somewhat, i would be interested to know how long it takes for yours





---------------------------------------------------------------------
feel free to correct my grammar, or any mistakes i make
---------------------------------------------------------------------
View user's profile View All Posts By User
Housane
Hazard to Others
***




Posts: 127
Registered: 3-9-2018
Location: Worcester, England
Member Is Offline

Mood: Let’s make

[*] posted on 18-6-2020 at 00:05


Yeah sure,I will do an update in a year or so



Green QD's so far

Feel free to correct grammar or incorect knknowledge. We are all learning.
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 18-6-2020 at 03:00


This sounds a lot like making levulinic acid.
View user's profile View All Posts By User
mackolol
Hazard to Others
***




Posts: 459
Registered: 26-10-2017
Member Is Offline

Mood: Funky

[*] posted on 18-6-2020 at 04:07


And what's the chemistry behind it. What chemical is formed by heating sugar with HCl and then neutralising it?
View user's profile View All Posts By User
Housane
Hazard to Others
***




Posts: 127
Registered: 3-9-2018
Location: Worcester, England
Member Is Offline

Mood: Let’s make

[*] posted on 18-6-2020 at 05:14


The idea is you are breaking down the carbon and then slowly reforming it in such a way that lots of tiny particles are formed and this is what changes the colour of the UV light. Thought emporium has a video about them. The acid slightly alters this. Others colours should be possible in Basic solutions and the colour may change depending on what acid is used, more exeprimatation I need to do



Green QD's so far

Feel free to correct grammar or incorect knknowledge. We are all learning.
View user's profile View All Posts By User
Housane
Hazard to Others
***




Posts: 127
Registered: 3-9-2018
Location: Worcester, England
Member Is Offline

Mood: Let’s make

[*] posted on 18-6-2020 at 13:13


I think I have just made yellow quantum dots, I will post again when the solution is concentrated enough to get a good picture



Green QD's so far

Feel free to correct grammar or incorect knknowledge. We are all learning.
View user's profile View All Posts By User
wg48temp9
National Hazard
****




Posts: 789
Registered: 30-12-2018
Location: not so United Kingdom
Member Is Offline


[*] posted on 14-8-2020 at 14:21


While looking for a wiring diagram for my dishwasher, which I did not find, but I did find a paper describing how to make Doped/Co-Doped Carbon Quantum Dots. I thought others may find it useful so I am posting it in this thread.

Attachment: carbon-05-00024-v2.pdf (5.1MB)
This file has been downloaded 443 times




I am wg48 but not on my usual pc hence the temp handle.
Thank goodness for Fleming and the fungi.
Old codger' lives matters, wear a mask and help save them.
Be aware of demagoguery, keep your frontal lobes fully engaged.
I don't know who invented mRNA vaccines but they should get a fancy medal and I hope they made a shed load of money from it.
View user's profile View All Posts By User
Housane
Hazard to Others
***




Posts: 127
Registered: 3-9-2018
Location: Worcester, England
Member Is Offline

Mood: Let’s make

[*] posted on 11-10-2020 at 06:58


Ubya, I have just checked them and both the green and the yellow glow exactly the same as before



Green QD's so far

Feel free to correct grammar or incorect knknowledge. We are all learning.