Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: Can you store 95% sulfuric acid in HDPE for a long time?
NaK
Hazard to Self
**




Posts: 83
Registered: 12-9-2019
Member Is Offline


[*] posted on 10-2-2021 at 09:06
Can you store 95% sulfuric acid in HDPE for a long time?


I have some concentrated sulfuric acid that will hopefully last for many years, decades even. It is stored in HDPE currently but I noticed a bit of yellowing of the plastic in an older bottle. Will this hold up long term or do I need to rebottle it in glass? I really like the unbreakable nature of the plastics but I also don't want to have half of the bottle dissolved in the acid
View user's profile View All Posts By User
itsallgoodjames
Hazard to Others
***




Posts: 276
Registered: 31-8-2020
Location: America Lite
Member Is Offline


[*] posted on 10-2-2021 at 09:15


If the bottle or the acid is getting discoloured, you want a new bottle. You can get shatter resistant glass reagent bottles.



Nuclear physics is neat. It's a shame it's so regulated...

Now that I think about it, that's probably a good thing. Still annoying though.
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 10-2-2021 at 12:54


98% sulfuric acid, which I buy is poured into HDPE bottles.

This is a phosphoric acid, but sulfuric acid is in same 1L bottle.
received_1569655646559586.jpeg - 156kB received_2818146455100867.jpeg - 74kB




View user's profile View All Posts By User
Fyndium
International Hazard
*****




Posts: 1192
Registered: 12-7-2020
Location: Not in USA
Member Is Offline


[*] posted on 10-2-2021 at 23:34


They store sulfuric acid almost exclusively in HDPE canisters. I've always got mine in them, even the brand reagent grade ones. Never seen a glass bottle for it. Plastic, when allowed, is superior to glass in every way as a storage media.

If picking a new container, just make sure it is unadulterated HDPE, as many commercial plastics contain filler like calcium carbonate or other cheap stuff that lowers the bulk price of the plastic without affecting it's structural properties and allow it to be suitable for food packing and other not-too-reactive stuff, but may cause reaction with strong acids.

Sulfuric acid, especially technical grade ones, often comes naturally in slightly yellowish tint. Mine is at 98% pure, and it does not affect anything in any way.
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 10-2-2021 at 23:41


Mine is pure too. I can buy 95 or low concentrated sulfuric acid, which used in car batteries, but as you mentioned it has yellowish colour and i dont like this. I only have two technical reagents, first is calcium hypochlorite and ammonium nitrate from 50kg fertilizer packet.



View user's profile View All Posts By User
FrenchChemist
Harmless
*




Posts: 44
Registered: 25-1-2021
Member Is Offline


[*] posted on 15-4-2021 at 20:46


HDPE do the job for sulfuric, nitric also but for longer time only glass, maybe it was due to a faulty hdpe bottle art, nitric acid started to "condense" on the outside of the bottle, I had to transfer to the glass. After a year, nothing happens. Come on as I say maybe my HDPE container was defective
View user's profile View All Posts By User
woelen
Super Administrator
*********




Posts: 8150
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 15-4-2021 at 22:59


I also had sulfuric acid in HDPE bottles, but over time, the plastic became darker and darker grey. I decided to pour all acid in glass bottles. My acid is not slightly yellow or brown, it really is colorless like water, and in glass it remains that way.

Sulfuric acid, when sold for technical purposes, indeed usually is shipped in plastic bottles, but I also have a bottle of sulfuric acid, which is intended as a lab reagent. This is in a nice glass bottle, with a sturdy black cap, which has a white teflon liner inside.




The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
Sulaiman217
Harmless
*




Posts: 5
Registered: 8-5-2019
Location: Saudi Arabia
Member Is Offline

Mood: ionized

[*] posted on 16-4-2021 at 00:46


In my country you can buy 98% H2SO4 in almost all plumbing shop as drain opener. It is supplied in HDPE bottles. I bought 2 liters bottle back in the epedmic breakthrough ( around march 2020). I keep it in its bottle and frequently top up my Reagent bottle from it. Lately i am observing a slight discolor to the acid where it used to be very clear like water. That change in color never effected any reaction however.
View user's profile View All Posts By User
FrenchChemist
Harmless
*




Posts: 44
Registered: 25-1-2021
Member Is Offline


[*] posted on 16-4-2021 at 00:54


Yes, this PTFE liner are the best , so far i have storage problems only with PCl3 , but glass ampoule did the job or Schott DURAN Premium caps


Quote: Originally posted by woelen  
I also had sulfuric acid in HDPE bottles, but over time, the plastic became darker and darker grey. I decided to pour all acid in glass bottles. My acid is not slightly yellow or brown, it really is colorless like water, and in glass it remains that way.

Sulfuric acid, when sold for technical purposes, indeed usually is shipped in plastic bottles, but I also have a bottle of sulfuric acid, which is intended as a lab reagent. This is in a nice glass bottle, with a sturdy black cap, which has a white teflon liner inside.
View user's profile View All Posts By User
Belowzero
Hazard to Others
***




Posts: 187
Registered: 6-5-2020
Location:                 Member Is Offline
Member Is Offline


[*] posted on 16-4-2021 at 00:56


Quite often the caps are the weakest point.
And as mentioned above HDPE bottles tend to sweat over time.
I would vote against long time storage (years on end) of sulfuric acid in HDPE bottles.

Also I have a couple HDPE bottles of battery acid which seems to hold much better due to its lower concentration.

[Edited on 16-4-2021 by Belowzero]
View user's profile View All Posts By User
woelen
Super Administrator
*********




Posts: 8150
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 16-4-2021 at 01:08


Battery acid is no problem, the concentrated acid is (in the long run).
Concentrated HCl (37%) is a problem as well. The bottle gets wet on the outside. Even with 30% HCl this problem occurs, albeit less severely.

I store all my concentrated acids in glass bottles with suitable caps. I now have 4 liters of H2SO4, long term storage, which I keep, now that in the EU the concentrated acid cannot be purchased anymore. These 4 liters will last many years to come for me, and in those years they should remain nice waterclear as they are now. We now can buy 15% acid in 25 liter jerrycans for a little over EUR 1 per liter and I keep that in plastic, it is dilute and keeps well. Many experiments can be done with this 15% acid and the concentrated acid only is needed occasionally.

[Edited on 16-4-21 by woelen]




The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
greenlight
National Hazard
****




Posts: 796
Registered: 3-11-2014
Member Is Offline

Mood: Energetic

[*] posted on 18-4-2021 at 00:32


I have a large supply that has been stored for a decade now in black HDPE 15L jugs at about 15-25°C.
The only difference is it is much darker now after such a long time. Still functions as required and quickly carbonizes paper towel.





View user's profile View All Posts By User
Fyndium
International Hazard
*****




Posts: 1192
Registered: 12-7-2020
Location: Not in USA
Member Is Offline


[*] posted on 18-4-2021 at 09:54


I have also a HDPE bottle of 98% sulfuric acid over a decade old without single hint of issue.
View user's profile View All Posts By User
woelen
Super Administrator
*********




Posts: 8150
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 18-4-2021 at 11:03


For me, acid getting brown or darker IS an issue. It still may be fine for carbonizing paper or cleaning drains, but if you do experiments with e.g. transition metal complex formation, then any colored impurity is a big pain in the ass. So, for me, any container, which adds crap to my chemicals, is unfit for the purpose of storing that chemical. Some chemicals can be stored in nearly every container, while others require much more care in selecting a suitable container. Sulphuric acid is in the middle of the scale.



The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
Fyndium
International Hazard
*****




Posts: 1192
Registered: 12-7-2020
Location: Not in USA
Member Is Offline


[*] posted on 18-4-2021 at 11:25


I would just get a separate glass bottle for more special purposes and keep the rest of the 25 liters in a can. That's actually what I do with any stuff I got more than a bottle: I keep one bottle at hand for use, and refill it as needed from the drum. It's difficult to fill a 100mL cylinder from 25L canister anyway. Pun intended.

Quote: Originally posted by Sulaiman217  
In my country


How do you emigrate there? I'm getting tired of this shit.

[Edited on 18-4-2021 by Fyndium]
View user's profile View All Posts By User

  Go To Top