Reducing Cu and Ni with Zn


I read a blurb online about how zinc will not reduce nickel ions even though Zn is above Ni in the potential series.

https://www.nature.com/articles/142210a0

I thought this might be a useful way to separate copper from nickel, but I can't find any mention of it searching through the threads on that topic.

I decided to do a test and share what I did for feedback.

Here are two test tubes. The one on the left contains 1 mmol of CuSO4 and the one on the right contains 1 mmol of Ni2NO3.



Here are the same two test tubes one day after a slight excess of Zn dust was added.



The Cu test tube looks like all the Cu has reacted. To make any Cu ions more visible, I added 5 drops of 30% NH4OH. Here is a pic right after adding the ammonia before shaking,



and after shaking.



Am I right to conclude that the lack of visible blue means all the Cu has been reduced?

To see if any of the Ni was reduced, I used a neodymium magnet to try and move around the solid material in the Ni test tube. Here are pics I took while moving the magnet around the solid material. They're not the best pics because I twisted the tube between pics, but it was clear to me the solid material didn't move at all.





I think the next thing I'm going to do is try to plate the nickel out of solution. I'll update the post if I do.
View user's profile View All Posts By User
Fluorite
Hazard to Others
***




Posts: 139
Registered: 26-12-2018
Location: United Arab Emirates
Member Is Offline


[*] posted on 25-4-2021 at 14:23


You can also use aluminum to reduce nickel metal The reaction is not vigorous as with copper compounds but it happens
To see if there's any copper ions left in the solution you can bubble hydrogen sulfide or use sodium or ammonium sulfide to precipitate dark copper sulfide, zinc sulfide is white so it should not be a problem
View user's profile View All Posts By User
S.C. Wack
bibliomaster
*****




Posts: 2419
Registered: 7-5-2004
Location: Cornworld, Central USA
Member Is Offline

Mood: Enhanced

[*] posted on 25-4-2021 at 15:26


Zn reduces Ni salts, perhaps not quantitatively under all conditions or to pure Ni...with evolution of hydrogen...search term: Urushibara



"You're going to be all right, kid...Everything's under control." Yossarian, to Snowden
View user's profile Visit user's homepage View All Posts By User
electrokinetic
Hazard to Self
**




Posts: 52
Registered: 6-6-2012
Location: Rhuidean
Member Is Offline

Mood: No Mood

[*] posted on 25-4-2021 at 15:51


Quote: Originally posted by Fluorite  
You can also use aluminum to reduce nickel metal The reaction is not vigorous as with copper compounds but it happens
To see if there's any copper ions left in the solution you can bubble hydrogen sulfide or use sodium or ammonium sulfide to precipitate dark copper sulfide, zinc sulfide is white so it should not be a problem


Does the aluminum require any specific anion present to reduce the nickel? For example, aluminum foil put into copper sulfate won't do anything until chloride ions are added.
View user's profile View All Posts By User
symboom
International Hazard
*****




Posts: 1145
Registered: 11-11-2010
Location: Wrongplanet
Member Is Offline

Mood: Doing science while it is still legal since 2010

[*] posted on 25-4-2021 at 16:41


Not sure but I dissolved some pennies in peracetic acid and I'll deffinatly try the zinc trick to get the copper out
View user's profile View All Posts By User
njl
National Hazard
****




Posts: 609
Registered: 26-11-2019
Location: under the sycamore tree
Member Is Offline

Mood: ambivalent

[*] posted on 25-4-2021 at 17:08


Seeing as how many coins are simply a nickel/copper alloy, this might be a nice way to extract nickel from them.



Reflux condenser?? I barely know her!
View user's profile View All Posts By User
Bedlasky
International Hazard
*****




Posts: 1252
Registered: 15-4-2019
Location: Period 5, group 6
Member Is Offline

Mood: Volatile

[*] posted on 25-4-2021 at 20:31


Nickel react better with zinc or aluminium in the presence of chloride ions. Reaction is very fast and very exothermic (when I made nickel metal using aluminium and NaCl, reaction was so exothermic that I must cool the mixture). Nickel made by this way isn't pure even after several hours in concentrated NaOH (mine is 93,5% or so).



View user's profile View All Posts By User
electrokinetic
Hazard to Self
**




Posts: 52
Registered: 6-6-2012
Location: Rhuidean
Member Is Offline

Mood: No Mood

[*] posted on 25-4-2021 at 21:04


It is interesting that the Urushibara article specifically named NiCl2 as the nickel salt in the preparation of nickel using zinc.

Urushibara

What I am going to do tomorrow is add some chloride ions to the nickel nitrate test tube and report back what happens.
View user's profile View All Posts By User
electrokinetic
Hazard to Self
**




Posts: 52
Registered: 6-6-2012
Location: Rhuidean
Member Is Offline

Mood: No Mood

[*] posted on 25-4-2021 at 21:06


Quote: Originally posted by Bedlasky  
Nickel react better with zinc or aluminium in the presence of chloride ions. Reaction is very fast and very exothermic (when I made nickel metal using aluminium and NaCl, reaction was so exothermic that I must cool the mixture). Nickel made by this way isn't pure even after several hours in concentrated NaOH (mine is 93,5% or so).


Educate me please, what does the NaOH do purification-wise?
View user's profile View All Posts By User
S.C. Wack
bibliomaster
*****




Posts: 2419
Registered: 7-5-2004
Location: Cornworld, Central USA
Member Is Offline

Mood: Enhanced

[*] posted on 25-4-2021 at 21:27


Quote: Originally posted by electrokinetic  
It is interesting that the Urushibara article specifically named NiCl2 as the nickel salt in the preparation of nickel using zinc.


There is mention of using the sulfate in the related literature but it is generally not used for reasons which I haven't seen explained. The sulfate absolutely reacts...nitrate could possibly be reduced to ammonia.

[Edited on 26-4-2021 by S.C. Wack]




"You're going to be all right, kid...Everything's under control." Yossarian, to Snowden
View user's profile Visit user's homepage View All Posts By User
Bedlasky
International Hazard
*****




Posts: 1252
Registered: 15-4-2019
Location: Period 5, group 6
Member Is Offline

Mood: Volatile

[*] posted on 25-4-2021 at 21:28


NaOH remove leftover aluminium. Al react with NaOH to form [Al(OH)4]- and H2 gas. Nickel doesn't react with NaOH.

Chlorides help to proceed the reaction because of dissolving Al2O3 protective layer on the surface of aluminium (formation of [AlCl4]-). For zinc it is similar.




View user's profile View All Posts By User
electrokinetic
Hazard to Self
**




Posts: 52
Registered: 6-6-2012
Location: Rhuidean
Member Is Offline

Mood: No Mood

[*] posted on 25-4-2021 at 22:31


Quote: Originally posted by Bedlasky  
NaOH remove leftover aluminium. Al react with NaOH to form [Al(OH)4]- and H2 gas. Nickel doesn't react with NaOH.

Chlorides help to proceed the reaction because of dissolving Al2O3 protective layer on the surface of aluminium (formation of [AlCl4]-). For zinc it is similar.


Jesus Christ, I can't believe I had to ask that—I've used that reaction to make hydrogen for fire balloons. Thanks for clarifying though.
View user's profile View All Posts By User
electrokinetic
Hazard to Self
**




Posts: 52
Registered: 6-6-2012
Location: Rhuidean
Member Is Offline

Mood: No Mood

[*] posted on 30-4-2021 at 11:48


Here is the test tube a day after adding ten drops of saturated sodium chloride solution. There appears to be no change:



Right after adding a strip of aluminum foil:



And then 3 days later, where there does seem to be some cloudy material near the bottom. Test with a magnet for nickel was negative:


View user's profile View All Posts By User