Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: Heteropolymetalates
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 20-6-2022 at 03:07
Heteropolymetalates


Hello! I started making different Heteropolymetalates.


Today I made ammonium 12-molybdatecerate(IV) - (NH4)8CeMo12O42*8H2O. According to the methodology it is prepared as follows. However I did three times as much.

Add 7g of Ceric ammonium nitrate in 140ml water. add 30g of ammonium heptamolybdate tetrahydrate in 100ml watar. stirring is required. When the solution is mixed, a yellow precipitate is released.



288173839_1216685345733673_3738040980393290042_n.png - 1.5MB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 20-6-2022 at 04:48


Ammonium 6-molybdochromate(III) - (NH4)3[CrMo6O24H6] •nH2O. n= 4-7.

Dissolve 12 g of NH4Cr(SO4)2 •12H2O in 50ml H2O. Add 30 g ammonium heptamolybdate tetrahydrate in 110ml water. The solution will have a green color. It is necessary to add sulfuric acid until pH=4.5. A precipitate will then form which will have a purple color

received_751791049157067.jpeg - 190kB received_600554548078744.jpeg - 400kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 20-6-2022 at 22:30


Ammonium 6-molybdonickelate(II) - (NH4)4[NiMo6O24H6]•5H2O

Dissolve 22g of ammonium heptamolybdate tetrahydrate in 200 ml water and 2.6 g of nickel sulfate hexahydrate in 150 ml water. Mix the solutions and boil for 10 minutes.


received_599924564686928.jpeg - 293kB



received_1598903000490942.jpeg - 407kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 21-6-2022 at 01:06


three jars of phosphotungstic acid.


287313659_710989460195266_3858836210957485054_n.jpg - 420kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 21-6-2022 at 01:09


1L jar of phosphomolybdic acid.


287749860_526849902512331_1274553159076686319_n.jpg - 533kB




View user's profile View All Posts By User
Bedlasky
International Hazard
*****




Posts: 1253
Registered: 15-4-2019
Location: Period 5, group 6
Member Is Offline

Mood: Volatile

[*] posted on 21-6-2022 at 03:46


Hi Vano!

Hexamolybdatonickelate is labile at temperatures higher than 60 °C. Let it precipitate at room temperature, you will get light blue solid.

Solubility of heteropolymolybdates is much higher in hot water, it is better to cool down solution in the fridge. More precipitate will crush out.
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 21-6-2022 at 05:11


Hello and thanks! I didn't know that fact about Hexamolybdatonickelate, i just made it according old soviet book. I also made Silver phosphovanadate. Brown-black compound. When it dries I will post photos.



View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 21-6-2022 at 05:14


(NH4)8CeMo12O42*8H2O. I made more.

received_5507888439235188.jpeg - 244kB




View user's profile View All Posts By User
Bedlasky
International Hazard
*****




Posts: 1253
Registered: 15-4-2019
Location: Period 5, group 6
Member Is Offline

Mood: Volatile

[*] posted on 21-6-2022 at 13:19


Btw. tungstates can stabilize metal ions in high oxidation state (Mn(IV), Co(III), Ni(III), Pr(IV) etc.). Maybe molybdates can do the same? I don't know, never read about it, but I once made some solution containing Co(III) in excess of molybdate.
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 22-6-2022 at 03:28


There is also nickel(IV) heteropolymetalate in my book. I will try to get it in the near future.



View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 28-6-2022 at 02:27


silver 12-vanadophosphate Ag7(PV12O36)•nH2O f

288528282_439600207710288_430183686370274811_n.jpg - 301kB 289036884_813754186259846_7437827010735913754_n.jpg - 693kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 1-7-2022 at 21:32


Sodium 6-molybdoiodate. Na5(IMo6O24)•nH2O (n=26,34).


received_537569308049948.jpeg - 640kB

[Edited on 2-7-2022 by vano]




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 5-7-2022 at 00:25


Sodium 6-molybdocobaltate(III) - Na3(Mo6O24H6)*8H2O

290697578_417394350336447_6362229316556600263_n.jpg - 317kB

291001683_627837428252778_4182576376802180482_n.jpg - 272kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 5-7-2022 at 06:50


Na9[α-SbW9O33]*27H2O

290880456_798174408014037_3685426718766913404_n.jpg - 495kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 5-7-2022 at 08:29


Ammonium 12-molybdophosphate - (NH4)3[PMo12O40] *nH2O.

290777898_564228008676864_7144083088687137029_n.jpg - 764kB




View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4743
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: Seeking gainful employment

[*] posted on 5-7-2022 at 08:49


Beautiful! I especially like the Co(III) one. I haven't seen a green cobalt compound before as far as I can remember. Do you have any further experiments in mind for these products, or are you just making them all for your collection?



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 5-7-2022 at 09:29


Quote: Originally posted by Texium  
Beautiful! I especially like the Co(III) one. I haven't seen a green cobalt compound before as far as I can remember. Do you have any further experiments in mind for these products, or are you just making them all for your collection?


I haven't read anything specifically about the use of this compound, but if I see any information and am interested, I will try it. This time I just made it for my collection, I think when I make many other heteropolymetalates I will start to study their properties.





View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 7-7-2022 at 03:45


Cesium 12molybdic acid 1- silicate Cs2[SiMo12O39] * nH2O

Brauer p.1729-1730.

291035109_458774202742805_5020118966605750843_n.jpg - 487kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 26-7-2022 at 00:45


just nice photo

290311809_1216382395793911_7628062883029979986_n.jpg - 349kB




View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 14-8-2022 at 06:48


Potassium 6-molybdochromate(III) - K3[CrMo6O24H6] • nH2O


IMG-0883.jpg - 2.6MB
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 8-9-2022 at 08:05


Ammonium 10-molybdodicobaltate(III) - (NH4)6(Co2Mo10O30)*10H2O

IMG-2262.jpg - 1.2MB

color isn't very different from Na3(CoMo6O24H6)*8H2O.

IMG-2261.jpg - 1.5MB
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 10-10-2022 at 09:03


12-Molybdic Acid-1-Arsenate - H3[AsO4(Mo3O9)4] *nH2O

(Brauer - p. 1734)

IMG-2564.jpg - 2.3MB
IMG-2568.jpg - 1.7MB




View user's profile View All Posts By User
bob800
Hazard to Others
***




Posts: 240
Registered: 28-7-2010
Member Is Offline

Mood: No Mood

[*] posted on 21-10-2022 at 18:33


Awesome pics, love the bright yellow ones especially.

Keep it up!
View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 24-10-2022 at 09:08


Thank you!



View user's profile View All Posts By User
samarium14
National Hazard
****




Posts: 661
Registered: 22-3-2019
Location: Georgia
Member Is Offline


[*] posted on 29-10-2022 at 00:57


ammonium nonanmolybdatomanganate - (NH4)6[MnMo9O32]*nH2O


IMG-2754.jpg - 1.3MB




View user's profile View All Posts By User