SiO2 + Na thermite reaction?
I was curious, the typical amateur synthesis of making elemental silicon is via the thermite process using aluminum. But then you have to remove the
aluminum products, so typically people add sulfur to make that easier, but end up making some nasty fumes.
I was thinking, could I just melt some sodium metal, mix in the SiO2 to make the thermite mix (that way I don't have to deal with milling sodium and
have to fuss around with argon atmospheres and such)
That way all the products I don't want should be water soluble.
How many issues do you see with this before I start investing any time on it?
|
|
|
j_sum1
Administrator
      
Posts: 6472
Registered: 4-10-2014
Location: Limbo
Member Is Offline
Mood: Just got through yet another "take this job and shove it" moment.
|
|
You will probably have a problem with the Na boiling away.
I have not checked the thermodynamics either. But I think it will be energetically favourable.
Nothing wrong with trying though.
I have used Mg powder to make Si. It gets around the problem of boiling. The products are soluble in water. And use of Mg has a better delta H than
Na. Not to mention that it is cheaper and more accessible. You might want to consider that option.
|
|
|
Rainwater
National Hazard
  
Posts: 993
Registered: 22-12-2021
Member Is Offline
Mood: Break'n glass & kick'n a's
|
|
Not sure sodium metal will work for silicon. Its the primary component of glass and does not get attacked it by sodium in anhydrous conditions.
| Code: | SiO2 + 4 Na = 2 Na2O + Si
T = 0C
ΔH 69.5381 kJ/mol
ΔS -108.8677 J mol/K
ΔG 99.2753 kJ/mol
T=1000c
ΔG 208.1430 kJ/mol
|
"You can't do that" - challenge accepted
|
|
|
Admagistr
Hazard to Others
 
Posts: 395
Registered: 4-11-2021
Location: Central Europe
Member Is Offline
Mood: The dreaming alchemist
|
|
I would try it,but I see a problem in that the sodium would ignite in the air before attacking the SiO2.Therefore I would cover the reaction mixture
with a layer of NaCl.
|
|
|
NickBlackDIN
Harmless
Posts: 13
Registered: 10-5-2023
Member Is Offline
|
|
J_sum1:
I did think about Mg, but I didn't think MgO was water soluble.
the Na boiling away is a good point, I personally thought the bigger problem would be it just not getting hot enough for it to start taking the Oxygen
from the silicon. (Which I guess is the same problem)
Rainwater;
Ohh, good point, I didn't think about it that way. Though in glassmaking, isn't it usually sodium ions that are added? Not the metal?
Admagistr:
Ohh, that's not a bad idea to try and increase yield (assuming it even works in the first place)
We'll see how busy I am next long weekend whether or not I have the time to try it 
-----
Thank you folks for all the replies!
|
|
|
BromicAcid
International Hazard
   
Posts: 3323
Registered: 13-7-2003
Location: Wisconsin
Member Is Offline
Mood: Rock n' Roll
|
|
Lithium will undergo a sustained reaction with glass.
|
|
|
B(a)P
International Hazard
   
Posts: 1139
Registered: 29-9-2019
Member Is Offline
Mood: Festive
|
|
It converts to hydroxide with the addition of water. You could wash your silicon with an appropriate acid to get rid of the magnesium hydroxide/oxide.
Edit
Typo
[Edited on 12-7-2023 by B(a)P]
|
|
|
Admagistr
Hazard to Others
 
Posts: 395
Registered: 4-11-2021
Location: Central Europe
Member Is Offline
Mood: The dreaming alchemist
|
|
Quote: Originally posted by B(a)P  |
It converts to hydroxide with the addition of water. You could wash your silicon with an appropriate acid to get ride of it. |
Magnesium works very well, but the purity of the silicon obtained this way will not be high, some of the Si will certainly form some silicide with Mg,
which will be very difficult to clean from silicon with acid.Sodium would probably provide a purer product.
[Edited on 12-7-2023 by Admagistr]
[Edited on 12-7-2023 by Admagistr]
|
|
|
B(a)P
International Hazard
   
Posts: 1139
Registered: 29-9-2019
Member Is Offline
Mood: Festive
|
|
Quote: Originally posted by Admagistr  | Quote: Originally posted by B(a)P  |
It converts to hydroxide with the addition of water. You could wash your silicon with an appropriate acid to get ride of it. |
Magnesium works very well, but the purity of the silicon obtained this way will not be high, some of the Si will certainly form some silicide with Mg,
which will be very difficult to clean from silicon with acid.Sodium would probably provide a purer product.
[Edited on 12-7-2023 by Admagistr]
[Edited on 12-7-2023 by Admagistr] |
Won't magnesium silicide react rapidly with a mineral acid to form silane? Making sure you do not have an excess of magnesium should reduce the
magnesium silicide.
|
|
|
Admagistr
Hazard to Others
 
Posts: 395
Registered: 4-11-2021
Location: Central Europe
Member Is Offline
Mood: The dreaming alchemist
|
|
Won't magnesium silicide react rapidly with a mineral acid to form silane? Making sure you do not have an excess of magnesium should reduce the
magnesium silicide.
[/rquote]
If the Mg silicide is dispersed in the silicon, the reaction will probably not be very fast...But the silicon could be finely pulverized...Another
impurity in Si will be unreacted SiO2.
|
|
|
averageaussie
Hazard to Self

Posts: 93
Registered: 30-4-2023
Location: Right behind you
Member Is Offline
Mood: school
|
|
[/rquote]
Another impurity in Si will be unreacted SiO2.[/rquote]
Could melting the bulk silicon in an inert atmosphere make the silica sink in the liquid silicon? silica has a density of 2.65 g/cm3, and liquid
silicon has a density of 2.57 g/cm3.
I know that melting the silicon might be a pain, but I see no other way to remove SiO2 impurities without turning your silicon to dust and picking it
out.
even then, SiO2 impurities aren't even that visible I think, nor do they interfere with a reaction.
|
|
|
metalresearcher
National Hazard
  
Posts: 822
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
I tried reacting SiO2 with Mg powder, it is a (rather slow) sustainable reaction, it gets very hot and then I dump it into HCl solution to dissolve
MgO.
But indeed, melting the reaction result is a pain, not particularly because of the required 1410 C temperature (can be reached in a propane / air
furnace or with a carbon arc of a welder), but the air. It oxidizes very quickly, hence the chip manufacturers use vacuum or inert gas (Ar) furnaces
to handle liquid Si in the Czochralski process to purify it.
|
|
|
averageaussie
Hazard to Self

Posts: 93
Registered: 30-4-2023
Location: Right behind you
Member Is Offline
Mood: school
|
|
Quote: Originally posted by metalresearcher  | I tried reacting SiO2 with Mg powder, it is a (rather slow) sustainable reaction, it gets very hot and then I dump it into HCl solution to dissolve
MgO.
But indeed, melting the reaction result is a pain, not particularly because of the required 1410 C temperature (can be reached in a propane / air
furnace or with a carbon arc of a welder), but the air. It oxidizes very quickly, hence the chip manufacturers use vacuum or inert gas (Ar) furnaces
to handle liquid Si in the Czochralski process to purify it. |
what setup do you have to melt the silicon? do you have access to an air free method of melting it?
also, can you post an image of the silicon obtained? I am quite curious about what it looks like.
|
|
|
Admagistr
Hazard to Others
 
Posts: 395
Registered: 4-11-2021
Location: Central Europe
Member Is Offline
Mood: The dreaming alchemist
|
|
Quote: Originally posted by averageaussie  | [/rquote]
Another impurity in Si will be unreacted SiO2.[/rquote]
Could melting the bulk silicon in an inert atmosphere make the silica sink in the liquid silicon? silica has a density of 2.65 g/cm3, and liquid
silicon has a density of 2.57 g/cm3.
I know that melting the silicon might be a pain, but I see no other way to remove SiO2 impurities without turning your silicon to dust and picking it
out.
even then, SiO2 impurities aren't even that visible I think, nor do they interfere with a reaction. |
An interesting aspect of fusing Si with SiO2 is the formation of SiO,which is volatile,hence one could probably remove SiO2 from silicon in this way!
|
|
|
metalresearcher
National Hazard
  
Posts: 822
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
Quote: Originally posted by averageaussie  |
what setup do you have to melt the silicon? do you have access to an air free method of melting it?
also, can you post an image of the silicon obtained? I am quite curious about what it looks like. |
No, I don't have access to it, but here a video of the reaction of Mg powder with silica sand. Afterwards I dumped it into HCl solution to dissolve
the MgO.
https://www.metallab.net/jwplayer/video.php?f=/forums/MgO-Si...
|
|
|
averageaussie
Hazard to Self

Posts: 93
Registered: 30-4-2023
Location: Right behind you
Member Is Offline
Mood: school
|
|
[/rquote]
No, I don't have access to it, but here a video of the reaction of Mg powder with silica sand. Afterwards I dumped it into HCl solution to dissolve
the MgO.
https://www.metallab.net/jwplayer/video.php?f=/forums/MgO-Silicon-20230817.mp4[/rquote]
with all those sparks, that would make quite the sparkler, no?
|
|
|
Rainwater
National Hazard
  
Posts: 993
Registered: 22-12-2021
Member Is Offline
Mood: Break'n glass & kick'n a's
|
|
| Quote: | | could I just melt some sodium metal, mix in the SiO2 to make the thermite |
I want to say I have confirmed that this reaction will not take place. But dont trust me, im an idiot
So today i tried sodium metal and finely ground SiO2 that i made from my stock of waterglass.
At about 875ish c under argon the sodium began to boil and made one hell of a mess.
But after boiling to dryness, i had no noticeable change in the weight of my crusable + sand.
Just the 5.02g loss which matches the weight of sodium added.
One observation was the mass of sand had fused together inside the crusable.
Which tends to happen with finely powered materials.
this is my first time heating amorphous silicate, i am not familiar with its properties
or behaviors. But with a melting point almost twice the reaction temperature i
wonder what flux like effect the molten sodium had. As some carbon from the crusable
did get mixed into the sand, it was easily removed by heating under oxidizing flame and
produced no noticeable change in mass after being removed with fire
Did i mention how much of a mess this made. Like how do i without a water hose even attempt... fKit i like fireworks
"You can't do that" - challenge accepted
|
|
|
BromicAcid
International Hazard
   
Posts: 3323
Registered: 13-7-2003
Location: Wisconsin
Member Is Offline
Mood: Rock n' Roll
|
|
Pretty sure magnesium silicides are made easily using Mg as a reluctant for SiO2 or perhaps that was how they were originally made. Might want to
look into it.
|
|
|
teodor
International Hazard
   
Posts: 1169
Registered: 28-6-2019
Location: Netherlands
Member Is Offline
|
|
Hm, is it exactly how Humphry Davy first get it? By heating SiO2 whith Na or K if I am not mistaken. I have his book in a different house, I will
update here with the detais.
Update:
Yes, I was right, it was Davy who first get the Si element by adding K to white-heated amorphouse modification of silica, detailed method of
preparation of which from a quarz sand takes a page in a book. But "compound is formed consisting of silica and potassa, and black particles not
unlike plumbago are found diffused through the compound". So, the yield of this method is not good and purity is not the best.
The first practical process (end of 19 century) used K2SiF6 instead of SiO2 to fuse it sith K or Na and leaching fluorides with water leaving Si as a
powder.
So, the answer, you cannot get it from SiO2 except in very small quantity.
[Edited on 10-2-2025 by teodor]
|
|
|
metalresearcher
National Hazard
  
Posts: 822
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
Magnesium is easier. Recently I did it again, a kind of thermite with Mg powder and silica sand.
The output can just be dissolved in an HCl solution.
https://www.metallab.net/jwplayer/video.php?f=/forums/Silico...
|
|
|
teodor
International Hazard
   
Posts: 1169
Registered: 28-6-2019
Location: Netherlands
Member Is Offline
|
|
J.W.Mellor, vol. VI. You can find it in the sciencemadness library. Contains description of many methods including Mg. But Mg route is not as simple
if you need 90%+ Si and not Si+MgSi. Also sometimes you can get an explosion with Mg. Read in Mellor.
|
|
|
Rainwater
National Hazard
  
Posts: 993
Registered: 22-12-2021
Member Is Offline
Mood: Break'n glass & kick'n a's
|
|
First hit on google
| Quote: | | French chemists Joseph Louis Gay-Lussac and Louis Jacques Thénard probably prepared impure amorphous Silicon by heating potassium with silicon
tetrafluoride. |
I was using sodium metal and silicon dioxide
"You can't do that" - challenge accepted
|
|
|
teodor
International Hazard
   
Posts: 1169
Registered: 28-6-2019
Location: Netherlands
Member Is Offline
|
|
Quote: Originally posted by Rainwater  | First hit on google
| Quote: | | French chemists Joseph Louis Gay-Lussac and Louis Jacques Thénard probably prepared impure amorphous Silicon by heating potassium with silicon
tetrafluoride. |
I was using sodium metal and silicon dioxide |
Do you know what is amorphous silicon?
The first crystalline silicon was prepared and analysed by the same man who first prepared potassium and sodium metals and exactly from silicon
dioxide, by the same principle, but with more success his experiment was with isolating boron which he get in a good yield from boron oxide. He tried
to use the same principle, also his goal was to show that silica is not an element but a complex compound with oxigen. Don't credit Lussac with all
that.
And I cited his own explanation why the result with isolating Si from SiO2 was not satisfactory by his own opinion as well as that he succeeded with
amorphous SiO2, not sand.
Well, of course you think that Google knows more.
|
|
|
Rainwater
National Hazard
  
Posts: 993
Registered: 22-12-2021
Member Is Offline
Mood: Break'n glass & kick'n a's
|
|
Sounds rude.
Google does know more than me.
No arguments to be made there.
As i said, im an idiot
So for a little more detail.
I slowly bubbled garage grade CO2 gas into a diluted solution of sodium rich sodium silicate containing the equilivent of 3 grams of
SiO2.
I misplaced a decimal point and added 10x times the amount i wanted to.
I was attempting to lower the free NaOH content.
this produced amorphous silicon dioxide as a very fine almost colloidal suspension.
Dangerous stuff, like the kind that causes silicosis.
I had nothing better to do, and needed to test out my new Frankensteined smelter, now with controled atmosphere. Trying to breach 2000c.
And remembered this discussion, so test I did, results i shared
"You can't do that" - challenge accepted
|
|
|
teodor
International Hazard
   
Posts: 1169
Registered: 28-6-2019
Location: Netherlands
Member Is Offline
|
|
I think you can get some reduction by dropping of small portions of 2000C+ amorphous silica into molten alkali or NaK. The mass of alkali will
dessipate the heat. Otherwise you should react SiO2 with gaseous metal, which is intetesting, of course, but requires a lot of work of appropriate
apparatus design. At this temperature usage of H2 or other gazeous staff could be as well effective and dangerous.
But taking into account the danger of explosion as well as consideration that amorphous calcined SiO2 is a very fine dust, K2SiF6 + Na route looks
more friendly. If your most interest is a thermite reaction, I think F2 is not less active as an oxidiser for this.