Author: Subject: Make Potassium (from versuchschemie.de)
oberkarteufel
Hazard to Self
**




Posts: 55
Registered: 11-12-2018
Member Is Offline

Mood: Mayonesium sulfate

[*] posted on 14-5-2019 at 00:54


Thank you for your answer. Currently I don't have an access to (or rather, excess money to spend) these alcohols, so in the fortunate event I have the place again to work further on this reaction I will rather try again the menthol, changing other variables.

I've checked all nearby stores (and some further ones) and all brands of "hypoallergenic" baby oil contained things like vitamins, palmitate esters, etc. Thus, liquid paraffin I used looks like the best option, since it's reasonably pure, cheap and available in virtually every pharmacy.

I also want to strongly encourage you to try this reaction.
View user's profile View All Posts By User
DavidJR
National Hazard
****




Posts: 908
Registered: 1-1-2018
Location: Scotland
Member Is Offline

Mood: Tired

[*] posted on 14-5-2019 at 03:39


Quote: Originally posted by oberkarteufel  
Thank you for your answer. Currently I don't have an access to (or rather, excess money to spend) these alcohols, so in the fortunate event I have the place again to work further on this reaction I will rather try again the menthol, changing other variables.

I've checked all nearby stores (and some further ones) and all brands of "hypoallergenic" baby oil contained things like vitamins, palmitate esters, etc. Thus, liquid paraffin I used looks like the best option, since it's reasonably pure, cheap and available in virtually every pharmacy.

I also want to strongly encourage you to try this reaction.


I tried making potassium with KOH, menthol, and baby oil and it didn't work. The baby oil I bought does claim to be hypoallergenic but according to the ingredients it contains isopropyl myristate and "parfum" (god knows what that is).
View user's profile View All Posts By User
walruslover69
Hazard to Others
***




Posts: 243
Registered: 21-12-2017
Member Is Offline

Mood: No Mood

[*] posted on 14-5-2019 at 09:00


I have tried with walmart brand hypoallergenic baby oil with some sort of fragrance with baffling results. The first attempt it went perfectly with maybe 5g of potassium being synthesized, but i have never been able to replicate the results. The second time huge plumes of white fog (not smoke) were generated after it reached ~150C. My 3rd and 4th attempts were very similar to what you reported with nothing happening except the oil turning a tan or light brown color.
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 14-5-2019 at 21:11


I'm pretty sure the white fog or smoke is the parfum being boiled out as it was when I tried baby oil heating baths.

[Edited on 15-5-2019 by draculic acid69]
View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 15-5-2019 at 05:51


Has anyone else reported success with menthol? I don't recall that being used for this before.
It's good practice to start by replicating a known successful process first, then trying modifications.
View user's profile Visit user's homepage View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 15-5-2019 at 06:12


Are you completely unaware of nurdrages research into sodium production using the same rxn as the KOH method above?
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 15-5-2019 at 06:20


If you aren't here's where it's at: NaOH/mg in baby oil w/menthol catalyst= Na metal.
People are now trying to make potassium with menthol catalyst. Pok has made rubidium and nurdrage is trying to do lithium with the same rxn.my theory is K might be too big to fit on the menthol molecule the way sodium does and the steric hindrance is affected.might have too stick to tertiary alcohols for K formation.
View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 15-5-2019 at 06:23


Not at all. I haven't watched every video though; does he succeed with menthol in one of them? That would have been more helpful information than a personal attack.

Even if he did use menthol for sodium, that doesn't necessarily prove it will work for potassium.


Edit: I didn't see your second post. Thank you, that is much more valuable information. I'll have to watch the newer videos.

[Edited on 5-15-2019 by MrHomeScientist]
View user's profile Visit user's homepage View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 15-5-2019 at 06:31


Glad to be of help,yes he succeeded with menthol. If you watch all of his sodium videos it spells out the mechanism what works what doesn't etc etc.
View user's profile View All Posts By User
oberkarteufel
Hazard to Self
**




Posts: 55
Registered: 11-12-2018
Member Is Offline

Mood: Mayonesium sulfate

[*] posted on 3-12-2019 at 04:08
Success!


Well, for longer I've been away from this topic than expected, but I'm back with some new results.
I have tried t-amyl alcohol as a catalyst...
... and well it worked!

DSC_1108.jpg - 141kB

I am also now sure that I have issues with insufficient power output of my hotplate. With a lot of hassle I was able to produce only these little droplets of metalic potassium. Well, at least that's something.
I am inclined to think that either menthol isn't a suitable catalyst for producing potassium or that it is much less active than t-amyl alcohol. Shame, because it's cheaper and easier to get... Anyway - achievement unlocked ;)
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 3-12-2019 at 19:34


Nicely done.did u perform everything the same as the unsuccessful menthol runs?
View user's profile View All Posts By User
oberkarteufel
Hazard to Self
**




Posts: 55
Registered: 11-12-2018
Member Is Offline

Mood: Mayonesium sulfate

[*] posted on 4-12-2019 at 03:11


Yup, same paraffin oil from pharmacy, heating regime etc. IIRC Total time of heating (first for drying the mixture, then after adding a catalyst) was 5+ hours.
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 4-12-2019 at 04:41


I think u just proved menthol doesnt work for potassium.
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6476
Registered: 4-10-2014
Location: Limbo
Member Is Offline

Mood: Just got through yet another "take this job and shove it" moment.

[*] posted on 20-12-2019 at 13:31


Quote: Originally posted by fotso  
Funny thing. The minute you posted it I also found out and was reading it :P
I immediately wanted to do this as well. However, I will make slight modifications, I will use i-PrOH instead of t-BuOH.
Also I don't know where to buy Shell D70 solvent, so i will use some high boiling hydrocarbon such as mineral turpetine.
I will still have to order some magnesium. I have some ribbon, I think i will use that to try it this weekend, but it's not enough to prepare more than a gram or two (I don't want to waste all the ribbon).

You are going to want a tertiary alcohol as a catalyst. So isopropyl alcohol will not work.
Also, I think scaling down to a couple of grams will be problematic. Mg ribon is cheap. But if you can get something clean with a better surface area, do so.
View user's profile View All Posts By User
elementcollector1
International Hazard
*****




Posts: 2689
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline

Mood: Molten

[*] posted on 20-12-2019 at 18:24


Shell D70 isn't really the most important part - kerosene/lamp oil works just as well. I personally couldn't make drugstore mineral oil work, though.



Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 20-12-2019 at 20:40


All the kerosene we get here in Australia is dyed blue which means distillation would be required.

[Edited on 21-12-2019 by draculic acid69]
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6476
Registered: 4-10-2014
Location: Limbo
Member Is Offline

Mood: Just got through yet another "take this job and shove it" moment.

[*] posted on 30-12-2019 at 05:32


I know it is a bit of a read, fotso. But these questions are answered within the thread. It is worth taking some time to go through it.

The tertiary alcohol (it must be tertiary) is a catalyst. The exact mechanism I forget but it is in here somewhere. Some limited success has been had with candle wax but there are other better choices. What seems to be critical is that it is alaphitic and that it has a high enough boiling point.

Happy reading.
View user's profile View All Posts By User
Pok
potassium Prometheus
***




Posts: 176
Registered: 5-12-2010
Member Is Offline


[*] posted on 2-1-2020 at 13:44


You are wasting your time. fotso just copies posts from other users.



View user's profile View All Posts By User
Abromination
Hazard to Others
***




Posts: 432
Registered: 10-7-2018
Location: Alaska
Member Is Offline

Mood: 1,4 tar

[*] posted on 15-2-2020 at 09:52


Did you read what j_sum said? It has to be tertiary, you cant use isopropanol. Isopropanol is a secondary alcohol.
Please read the thread.




List of materials made by ScienceMadness.org users:
https://docs.google.com/spreadsheets/d/1nmJ8uq-h4IkXPxD5svnT...
--------------------------------
Elements Collected: H, Li, B, C, N, O, Mg, Al, Si, P, S, Fe, Ni, Cu, Zn, Ag, I, Au, Pb, Bi, Am
Last Acquired: B
Next: Na
--------------
View user's profile View All Posts By User
Tsjerk
International Hazard
*****




Posts: 3040
Registered: 20-4-2005
Location: Netherlands
Member Is Offline

Mood: Mood

[*] posted on 15-2-2020 at 10:07


A catalyst boiling well below the reaction temperature in a liquid reaction is probably not a very good catalyst. Who would guess?

[Edited on 15-2-2020 by Tsjerk]
View user's profile View All Posts By User
Abromination
Hazard to Others
***




Posts: 432
Registered: 10-7-2018
Location: Alaska
Member Is Offline

Mood: 1,4 tar

[*] posted on 15-2-2020 at 10:50


Also it looks like he literally copied his first post from earlier in the thread.
Tertiary butanol works fine as a catalyst, this has been discussed extensively and doesn’t need further debate.




List of materials made by ScienceMadness.org users:
https://docs.google.com/spreadsheets/d/1nmJ8uq-h4IkXPxD5svnT...
--------------------------------
Elements Collected: H, Li, B, C, N, O, Mg, Al, Si, P, S, Fe, Ni, Cu, Zn, Ag, I, Au, Pb, Bi, Am
Last Acquired: B
Next: Na
--------------
View user's profile View All Posts By User
charley1957
Hazard to Others
***




Posts: 197
Registered: 18-2-2012
Location: Texas
Member Is Offline

Mood: Hotter than the hinges of Hell! Well, not yet, but fixing to be!

[*] posted on 5-3-2021 at 10:11


Two summers ago I ordered some tert-butanol and when it arrived it was liquid, as I expected an alcohol would be. Just the other day I was checking out my chemicals and found my tert-butanol had dried out, leaving a solid substance behind. So as I was researching how to reconstitute it, I was looking through its physical properties and found that it is normally a solid. So when I first received it, it was in the hottest part of the Texas desert summer, so it was above its melting point of about 80 degrees F. Well now it’s in the cold season and my lab is unheated so it is in its natural state. It hadn’t “dried out” at all. My lesson learned was to not assume anything and to not jump to any early conclusions.

[Edited on Mar03-5-2021 by charley1957]




You can’t claim you drank all day if you didn’t start early in the morning.
View user's profile View All Posts By User
isoPaarden
Harmless
*




Posts: 1
Registered: 25-7-2022
Member Is Offline


[*] posted on 25-7-2022 at 15:38


My K-Metal Synth looks a bit suss
Basically followed what DBX did but with a bubbler on top to monitor H2 production and I threw in a little K-Metal to dry it out (and protect the glassware)

Isopar as mineral oil
2mg Powdered Magnesium
10g KOH
Slice of K-Metal
Heated to 150deg C and held until H2 production slowed

Added 3mg Powdered Magnesium
Heated to 180deg C (just below reflux)
Added 2mL of T-Butanol in small additions (went blue here) over 30 mins

Raised to reflux (just over 180deg C) and held for about 1 hr (started going red/purple)

[Edited on 25-7-2022 by isoPaarden]

PXL_20220720_061431556.MP.jpg - 528kBPXL_20220720_061106016.jpg - 627kBPXL_20220720_060421734.jpg - 692kB
View user's profile View All Posts By User
Acetyl
Harmless
*




Posts: 2
Registered: 15-1-2024
Location: Poland
Member Is Offline

Mood: discoverer, student, scientist

[*] posted on 27-1-2025 at 16:14


Hi everyone, this is my first post over here.

I also attempted to obtain metallic potassium with different results. In total, I conducted 7 attempts, during which I obtained a lot of tiny potassium balls (mostly), in two attempts I obtained several large pieces of potassium. The last attempt ended in a total fiasco and I extracted absolutely nothing.

In a my the experiments I used Mg powder (Mg filings did not react), pure KOH (about 90% KOH content) and tert-butyl alcohol. As a solvent I bought 3 bottles of kerosene from three different stores. According to my experience, cosmetic kerosene (practically odorless) was the least useful, while I achieved the best results with illuminating kerosene.

02.jpg - 429kB 04.jpg - 362kB 05.jpg - 335kB 06.jpg - 437kB


Regardless of the outcome of the experiment, a lot of potassium always remained among the other reaction product: MgO (MgOH)2. This was visible when I cleaned the flat bottom flask using water. For those who will do this - when pouring water into the flask, hydrogen is rapidly released and ignited, causing strong explosions.

Apart from the fact that the kerosene was of different origin (EC no.: 918-481-9 was identical) and the composition also - C10-C13 alkanes with a content of aromatic compounds <2%. The equipment and conditions of the reaction were identical each time: maintaining the kerosene boiling for 4-4.5 h with frequent, intensive mixing of the content. The proportion of KOH/Mg/Terbutyl-OH according to the recipe, only as for the kerosene, I used a smaller amount than the patent recommends. Before adding the catalyst, the contents were always crushed with a steel rod. The reflux condenser was not plugged to prevent access of fresh air, but this did not seem to interfere with the reaction.

I have used 250g of KOH in total and the amount of potassium (covered with naphtha) was 50g, so the efficiency was ~30%. Poor.
09.jpg - 589kB 10.jpg - 448kB 07.jpg - 394kB 08.jpg - 620kB
View user's profile View All Posts By User
LesserLordKusanali
Harmless
*




Posts: 4
Registered: 25-3-2024
Member Is Offline

Mood: No Mood

[*] posted on 26-2-2025 at 13:14


Quote: Originally posted by mr.crow  
Here is something cool I found, not mine of course

http://www.versuchschemie.de/topic,14677,-Synthese+von+Kaliu...

Translation



The site is down now but I found a copy of the broken url on way back machine (https://web.archive.org/web/20120301222342/http://www.versuc...). I am interested if anyone has found any other catalysts for this reaction. I know that nurdrage found menthol but the reaction is much slower
View user's profile View All Posts By User