Strongly heating K2CO3 + C foams ?


In order to try a 19th century experiment (and commercial production of sodium with similar Na2CO3 + C in that era) I mixed some K2CO3 with powdered charcoal.
I put the mixture in a 316 stainless steel retort with its neck dipped in mineral oil. The same setup as I used successfully with KOH + Mg which indeed yielded some K balls in the oil.
Now I heated it to 1200 C (checked with an infrared pyrometer on the bright orange body of the retort) for a few minutes until bubbling ceased.
It was 21g K2CO3 and 3.5g charcoal powder.
The 316 stainless appears to be rather resilient even at 1200 C, but is is only for short times. It is still in good condition after several heats over 1000 C.

Above 1100 C this reaction takes place:

K2CO3 (liquid) + 2C (powder) => 2K (vapor) + 3CO (gas)
140 (21g) 24 (3.5g)

The threaded opening of the retort was sealed with Teflon tape which did work despite it decomposes (probably the carbon leftover) at such temperature. There were barely any leaks as I did not see flame discoloration due to purplish K+ ions.
After opening and dumping the retort into water I heard a few small explosions inside the tube but the top part was full of foamed stuff. Weird, because the lower (hot) part of the retort was only filled half full at the beginning with the charcoal powder with the pre-dried K2CO3 on top. Now it was empty. The top part contained black frozen foam.

What did actually happen ? It appears that the liquid K2CO3 started to foam with the charcoal powder as CO gas appears.
On the pictures, the furnace running and the retort after use.


furnace1.jpg - 946kB furnace2.jpg - 411kB retort.jpg - 1.8MB
View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 4-10-2025 at 07:21


How long did you heat it? Old book describe time of 12 hours and whithe glowing heat , first came burning gases over and at last the Potasium. They mention to use excess potash because it forms dangerous Potasiumcarbonmonoxide and black substance that explodes. With Sodium there is non such reaction. Maybe the black foam is this explosive substance?
Castner reduction with Ironcarbid (ironfillings heated with tar or very Carbonrich Iron) works on 800C and only 1 1/2 to 2 hours. That was the first industrial methode of making Alkali metals.


[Edited on 4-10-2025 by Alkoholvergiftung]

[Edited on 4-10-2025 by Alkoholvergiftung]
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 822
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 4-10-2025 at 07:55


I heated it a few minutes until the bubbling in the jar with oil stopped.
The Potasiumcarbonmonoxide story can be an explanation of the explosions I heard.
Maybe next time heating with excess K2CO3 ?

View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 4-10-2025 at 08:17


I would use the excess because more of the old sources state the danger of an explosible black potassium compound.
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 822
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 4-10-2025 at 08:27


Quote: Originally posted by Alkoholvergiftung  
I would use the excess because more of the old sources state the danger of an explosible black potassium compound.

Where did you get this info from ?
View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 4-10-2025 at 09:03


from the book: Darstellung Chemischer Preperate, and Metalle und ihre Reihndarstellung.
The yield was bad too 2-3 parts Potassium from 14 parts Potassiumcarbonat.
The book has an discription with pictures for the apperatus too. Mostly they used musket barrels as retorte. I think they are to many side to make photos and post it here and they are in german.
Oh and favorite starting material was Potassiumtartarat heated in an closed fessel with an lid so only an mix of carbon and potassiumcarbonat remains.

[Edited on 4-10-2025 by Alkoholvergiftung]
Castner reduced KOH with Ironcarbid an mistake i made bevore.
The book "Reine Metalle" labeld the black substance as potassiumcarbonyl.

[Edited on 4-10-2025 by Alkoholvergiftung]
View user's profile View All Posts By User
bnull
National Hazard
****




Posts: 994
Registered: 15-1-2024
Location: East Woods
Member Is Offline

Mood: Fecking annoyed

[*] posted on 4-10-2025 at 09:22


Is this Darstellung the one by Hugo Erdmann?



Quod scripsi, scripsi.

B. N. Ull

We have a lot of fun stuff in the Library.

Read The ScienceMadness Guidelines. They exist for a reason.
View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 4-10-2025 at 10:15


Its from Dr. G. C. Wittstein. Munic 1857.
View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 4-10-2025 at 10:36


You need to cool the condensor with ice water that what they wrote and the Stove (Destilling) system looked something like this.


Attachment: Kalium2.pdf (69kB)
This file has been downloaded 76 times

View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 4-10-2025 at 10:51


I ve put all files in one together hope it works this time.

Attachment: Kalium.pdf (542kB)
This file has been downloaded 73 times

View user's profile View All Posts By User
bnull
National Hazard
****




Posts: 994
Registered: 15-1-2024
Location: East Woods
Member Is Offline

Mood: Fecking annoyed

[*] posted on 4-10-2025 at 12:36


Thank you.

Edit: I found a copy of Darstellung at Internet Archive: https://archive.org/details/anleitungzurdars00witt/page/n3/m.... Potassium starts on page 423.

[Edited on 4-10-2025 by bnull]




Quod scripsi, scripsi.

B. N. Ull

We have a lot of fun stuff in the Library.

Read The ScienceMadness Guidelines. They exist for a reason.
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 822
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 5-10-2025 at 10:34


This old book (1844) is really interesting, some incorrect formulas (potassium oxide as KO instead of K2O and water HO).

Quote: Originally posted by Alkoholvergiftung  
You need to cool the condensor with ice water that what they wrote and the Stove (Destilling) system looked something like this.

This is a different and far more complex setup, in a simple setup this will clog the distiller as the K freezes in the pipe leading to the oil.
View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 238
Registered: 12-7-2018
Member Is Offline


[*] posted on 5-10-2025 at 11:26


The book is good because there are lot of tips what you could do wrong. I know that its outdated but if someone trys to make same basic chemicals by yourself this book is perfect.
Modener books write about Vakuumdestillation of CaC2 and KF or KF reduction with Mg (grieß). But who has an Vakuumdestillation setup for higher temperatures
View user's profile View All Posts By User