Ceramic substrate PbO2 electrode construction
This really belongs in Technochemistry, but I didn't want to create a new topic.
I found an (once you sift through the dribble) easy method to construct a ceramic substrate PbO2 anode in this patent (US 4,008,144):
4,008,144
[Edited on 18-8-2004 by vulture]
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
Finally I have obtained 1kg of copper carbonate, which I've converted to copper acetate with acetic acid. The MSDS for cupric acetate states that
skin irritation can be caused by skin contact. I just thought I should mention to anyone trying this out that skin irritation is just the first name.
It, in fact, itches like nobody's business! I'm going crazy, it itches like hell! Arrgghhh!!! (I know I shouldn't have gotten it on my
skin, but being the slobbering idiot I am.....)
[Edited on 2004-7-28 by axehandle]
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
Esplosivo
Hazard to Others
 
Posts: 491
Registered: 7-2-2004
Location: Mediterranean
Member Is Offline
Mood: Quantized
|
|
Pay attention when using such salts. Lead acetate is worse since it is readily absorbed through the skin, and I suppose none of us want an increased
lead concentration in the blood right 
Well anyway, I just wanted to ask you to document the separation of the formed PbO2 when you have oxidised the Pb acetate. Chemoleo told me he used
centrifugation, but I don't possess a large enough centrifuge to seperate resonable quantities of ppt. Filtration prooved useless, since most of
the PbO2 simply passed through the filter (but the reson surely is that I used a cheap coffee filter). Suggestions are welcome.
Theory guides, experiment decides.
|
|
|
jimwig
Hazard to Others
 
Posts: 215
Registered: 17-5-2003
Location: the sunny south
Member Is Offline
Mood: No Mood
|
|
isn't PbO2 that dark brown powder inside all these lead acid batteries I have been taking apart ?
I pretty sure it is.
|
|
|
Esplosivo
Hazard to Others
 
Posts: 491
Registered: 7-2-2004
Location: Mediterranean
Member Is Offline
Mood: Quantized
|
|
Yes it is. It might contain some lead sulphate though. Anyway that is the stuff.
Theory guides, experiment decides.
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
| Quote: |
Well anyway, I just wanted to ask you to document the separation of the formed PbO2 when you have oxidised the Pb acetate. Chemoleo told me he used
centrifugation, but I don't possess a large enough centrifuge to seperate resonable quantities of ppt. Filtration prooved useless, since most of
the PbO2 simply passed through the filter (but the reson surely is that I used a cheap coffee filter). Suggestions are welcome.
|
I sure will. Right now I have a vat containing 10 litres of water, 500g of copper carbonate converted to cupric acetate, and a huge chunk of lead. The
displacement is slow going, but it seems to work. I expect it to take a few weeks though.
Edit: (next day) The lead lump was half eaten through! Just dumped in a freshly cast ingot. This is faster than I thought.
[Edited on 2004-8-3 by axehandle]
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
JohnWW
International Hazard
   
Posts: 2849
Registered: 27-7-2004
Location: New Zealand
Member Is Offline
Mood: No Mood
|
|
Re: Pb compounds
I have several kilograms of metallic Pb lying around my place, in the form of old Pb pipes and roof flashing that was removed when I did some
renovations and alterations, along with fishing sinkers. Now I know what to do with it!
BTW: PbO2 and soluble plumbates e.g. Na2PbO3 are very powerful oxidants, capable of oxidizing Mn(II) to MnO4- in alkaline solution, and probably also
Fe(II) to FeO4--. MnO2 is much weaker.
Plumbate, and also bismuthate(V), are in fact used in a colorimetric method for determining Mn in water, by oxidation to MnO4-, the absorbance of
which in about the middle of the visible spectrum is then measured. However, it is interfered with by the presence of Fe, which is oxidized at the
same time to FeO4--, which has substantial absorbance in the same part of the visible spectrum.
John W.
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
There, the Pb(Ac)2 via copper carbonate --> copper acatate --> lead acetate route was successful. I'm right now boiling in the 10 litres of
water it was done in --- very boring.
What I noted was that the lead chunks in the vat were eaten up at a very satisfactory rate: over 1kg of solid lead was eaten up in 3 days! The
displaced copper doesn't stick, BTW, it falls to the bottom in small pieces; these were very easy to remove using a simple coffee filter.
The copper carbonate as obtained from my pottery supplier wasn't completely pure. Some insoluable junk, white to white-blue in color, it left at
the bottom of the vat. Hasn't interfered with the process though AFAIK.
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
JohnWW
International Hazard
   
Posts: 2849
Registered: 27-7-2004
Location: New Zealand
Member Is Offline
Mood: No Mood
|
|
I think that the best way of obtaining Pb(IV) for use as a reagent in solution is by firstly dissolving PbO (litharge, obtainable from plumbous salts
or heating finely divided metallic Pb in air), or else metallic Pb itself (with the evolution of hydrogen) in concentrated excess NaOH or KOH to form
plumbite, PbO2--; then electrolysis of an alkaline solution of this at an appropriate voltage to obtain a solution of plumbate, PbO3--. Na or K
bismuthate(V) is is obtained in a similar manner. Acidification of the solution at a low temperature with a strong mineral acid would precipitate out
PbO2.
It, and bismuthate, is used in colorimetric chemical analysis for Mn by oxidizing the latter to MnO4-, although any Fe present is also oxidized to
FeO4-- and interferes.
A commercial use of Na or K plumbate solution is to obtain Ca or Zn plumbates, which are used as corrosion-preventing metal paint primers especially
for galvanized iron, as precipitates by adding Ca or Zn salts.
I am rather surprised at the posts describing Pb dissolving in non-oxidizing acids like HCl, which should not happen in the absence of a strong
oxidant because Pb is below H in the electrochemical series. Perhaps it was not pure Pb, but solder? - the Sn content in it would dissolve in HCl.
John W.
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
No... Pb is ABOVE H in the electrochemical series, at least in my (handwritten) variant:
Li, K, Ba, Ca, Na, Mg, Al, Mn, Zn, Cr, Fe, Co,
Ni, Sn, Pb, H, Cu, Hg, Ag, Au, Pt
And Pb(Ac)2 is a lead(II) salt, not a lead(IV) salt....
And Pb doesn't dissolve in NaOH, I tried it 5 weeks ago.
Your post is making me confused, but it could be you (or me) being drunk. I know I am!
[Edited on 2004-8-14 by axehandle]
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
chemoleo
Biochemicus Energeticus
   
Posts: 3005
Registered: 23-7-2003
Location: England Germany
Member Is Offline
Mood: crystalline
|
|
Indeed, Pb does have a negative standard potential. Yet it doesnt dissolve in dilute acids (except HNO3), not even HF < 60%. It dissolves in hot
conc. H2SO4, forming a complex. But it does dissolve i.e. in HAc, in the presence of oxygen (slowly of course). Or HCl - although even slowlier
because PbCl2 is rel. insoluble.
Regarding your plumbate route - sure, that may well work - dissolution of any PbII salt in NaOH to form the [Pb(OH)4]2- ion, then electrolysis to
[Pb(OH)6]2-. This in turn has then to be converted to PbO2, presumably with an acid. Surely not as simple as simply adding alkaline NaOCl to PbII
salt.
Burning fine Pb - how realistic is that? HNO3- always the hassle with NOx and wasting HNO3. The copper acetate route sounds still best to me!
In case you misunderstood this JohnWW, the issue was about PbO2, not soluble PbIV compounds!
Never Stop to Begin, and Never Begin to Stop...
Tolerance is good. But not with the intolerant! (Wilhelm Busch)
|
|
|
JohnWW
International Hazard
   
Posts: 2849
Registered: 27-7-2004
Location: New Zealand
Member Is Offline
Mood: No Mood
|
|
Axehandle - where did you get your electrochemical series from, viz.:
Li, K, Ba, Ca, Na, Mg, Al, Mn, Zn, Cr, Fe, Co, Ni, Sn, Pb, H, Cu, Hg, Ag, Au, Pt ?
Some versions on the internet which I found by searching on Google for "electrochemical series" (using also -amazon -buy -purchase -payment
-price as negative search parameters to filter out book advertisements) put Pb just above H (by -0.13 volt), while others put Pb just below H.
In any case, even if the very small negative potential for Pb -> Pb++ over H of -0.13v is correct, this small potential, plus the poor solubility
of PbCl2, would result in the reaction of Pb with HCl being initially slow, and then arrested after a short time due to the layer of PbCl2, except at
high temperatures with an excess of HCl. Similarly, the solubility of PbSO4 in aqueous solution is even less, being infinitesimal even in boiling
water, which explains why the H2SO4 in lead-acid batteries does not simply dissolve away all the Pb.
(BTW They agree that Cr (-0.74v) and Ni (-0.24v) are above H, which means that the corrosion resistance of stainless steels, and of
"hastelloys" containing principally Cr and Ni, is due entirely to the formation of impervious oxide layers.)
John W.
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
| Quote: |
Axehandle - where did you get your electrochemical series from, viz.:
Li, K, Ba, Ca, Na, Mg, Al, Mn, Zn, Cr, Fe, Co, Ni, Sn, Pb, H, Cu, Hg, Ag, Au, Pt ?
|
A Swedish college chemistry testbook printed in 1960. I'm fairly sure my notes are correct, I usually double check when copying. Can't vouch
for the accuracy of the book though...
I'm ready to make PbO2 from the acetate now using NaOH + NaOCl (or KMnO4?), just wanted to ask those who have done this: The PbO2 precipitate
formed, does it sink to the bottom or float? (This is crucial for me to know...)
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
Esplosivo
Hazard to Others
 
Posts: 491
Registered: 7-2-2004
Location: Mediterranean
Member Is Offline
Mood: Quantized
|
|
It first forms as a sort of 'suspension' but after some time it settels on the bottom. I found it very difficult to extarct this ppt from
the liquid, filtering only resulted in the collection of a very small quantity of PbO2 as I said previously in this thread. Wish you all the luck you
will need
Theory guides, experiment decides.
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
That was what I was afraid of. I suppose adding only a stochiometrically balanced amount of oxidizer, and then separating the precipitated PbO2 by
sedimentation would be best then...
I'll see whether KMnO4 can oxidize Pb(OH)2 to PbO2, it would have the advantage of being its own colour indicator...
[Edited on 2004-8-18 by axehandle]
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
chemoleo
Biochemicus Energeticus
   
Posts: 3005
Registered: 23-7-2003
Location: England Germany
Member Is Offline
Mood: crystalline
|
|
Well, in principle it is quite simple nonetheless.
PbO2 is bound to have a high density, so it will settle rather quickly. Definitely faster than CaSO4, which is equallly a pain to filter.
So, I would mix/heat your solution with NaOCl, like in a large batch.
Then, using a high glass/ beaker, let teh products settle over night.
Decant.
Repeat this 2-3 times. Then boil the remaining water off, and put on a radiator to get rid off the last bits of water. You could resuspend this in H2O
(to get rid of traces of NaCl and such), and filter. I am sure the filtering wont be a problem then, the PbO2 clumps up and won't go into
suspension like before.
Alternatively I suggest a centrifuge ... then the waiting/decanting wont be necessary several times, but prob. only once 
Edit: As to the KMnO4 - I guess you ought to keep it basic, too. I am not sure whether you might get a precipiate of MnO2, so this might be mistaken
(or mix) for PbO2.
[Edited on 18-8-2004 by chemoleo]
Never Stop to Begin, and Never Begin to Stop...
Tolerance is good. But not with the intolerant! (Wilhelm Busch)
|
|
|
Polverone
Now celebrating 23 years of madness
       
Posts: 3191
Registered: 19-5-2002
Location: The Sunny Pacific Northwest
Member Is Offline
Mood: Chastened
|
|
I oxidized my Pb acetate in acetic acid with Ca(OCl)2. This formed a fairly easy-to-filter precipitate of PbO2, perhaps because I was using a
concentrated, solid oxidizer instead of a dilute aqueous solution. The calcium waste products dissolved in the acid. After the first filtration, I
washed the precipitate with water several times before letting it dry.
|
|
|
axehandle
Free Radical
   
Posts: 1065
Registered: 30-12-2003
Location: Sweden
Member Is Offline
Mood: horny
|
|
Thank you both for the suggestion of washing the mix repeatedly. Stupidly enough that was something I didn't even consider -- just goes to show
that I lack lab skill (or perhaps that I'm an idiot, I sure feel like one...)....
My PGP key, Fingerprint 5D96 E09E 365D 1867 2DF5 C2FE 4269 9C19 E079 CD35
\"Verbing nouns weirds the language!\"
|
|
|
JohnWW
International Hazard
   
Posts: 2849
Registered: 27-7-2004
Location: New Zealand
Member Is Offline
Mood: No Mood
|
|
KMnO4 cannot oxidize Pb(II) to Pb(IV), at least not under neutral or alkaline conditions. Pb(IV) is usually the stronger oxidant. In fact, a
colorimetric method of analysis for Mn in water involves oxidizing it to MnO4- with Na or K plumbate(IV) in alkaline solution. (It also oxidizes Fe to
FeO4--, which unfortunately interferes with the analysis).
As for oxidizing Pb(II) to a precipitate of PbO2 with Ca(OCl)2 ("chloride of lime" , which gives an alkaline solution: are you quite sure that you did not end up with calcium plumbate, CaPbO3, instead? If the precipitate
was light gray in color (which is the color of CaPbO3 primer paint for galvanized iron), this would be indicated.
John W.
|
|
|
Polverone
Now celebrating 23 years of madness
       
Posts: 3191
Registered: 19-5-2002
Location: The Sunny Pacific Northwest
Member Is Offline
Mood: Chastened
|
|
I applied this oxidizer to a solution of lead acetate in aqueous acetic acid, so the system was never alkaline. I obtained a heavy, dark brown powder.
|
|
|
S.C. Wack
bibliomaster
   
Posts: 2419
Registered: 7-5-2004
Location: Cornworld, Central USA
Member Is Offline
Mood: Enhanced
|
|
Check your books, John. McAlpine and Soule:
"PbO2...is formed...(b) by treating Pb(II) in alkaline soln with oxidation agents, as halogens, H2O2, KMnO4, NaOCl, etc."
EDIT: Hawley's: "PbO2...Derivation: By adding bleaching powder to an alkaline solution of lead hydroxide."
Merck: "PbO2...Lab prepn from Pb(II) acetate and Ca(OCl)2: Newell, Maxson, Inorg Syn 1, 45 (1939)"
[Edited on 18-8-2004 by S.C. Wack]
|
|
|
FrankRizzo
Hazard to Others
 
Posts: 210
Registered: 9-2-2004
Member Is Offline
Mood: No Mood
|
|
What about mixing with molten KNO3? Don't you end up with PbO and KNO2 (also useful)?
|
|
|
S.C. Wack
bibliomaster
   
Posts: 2419
Registered: 7-5-2004
Location: Cornworld, Central USA
Member Is Offline
Mood: Enhanced
|
|
Mixing what with nitrate?
I'll guess: PbO + NaNO3 -> PbO2 + NaNO2
However: 3 PbO + NaNO3 -> NaNO2 + Pb3O4
and:
3 Pb + 4 NaNO3 = Pb3O4 + 4 NaNO2
Pb3O4 + 4 HNO3 = 2 Pb(NO3)2 + PbO2 + 2 H2O
AFAIK, that 1st equation is better for PbO2 than nitrite.
|
|
|
chemoleo
Biochemicus Energeticus
   
Posts: 3005
Registered: 23-7-2003
Location: England Germany
Member Is Offline
Mood: crystalline
|
|
No, he meant Pb + KNO3 --heat--> PbO + KNO2.
The KNO2 is soluble in water, while PbO isn't.
It works, but it isn't a terribly economic method. Plus I wouldnt want to play around tooo much with molten KNO3 - unless of cause I was to
prepare KNO2 - for which there aren't many methods that are easier than this.
Edit: I am not entirely sure about whehter Pb3O4 is produced, if Pb is added to molten KNO3. At least I haven't heard of it. I guess, as usual
it's a question of conditions.
[Edited on 20-8-2004 by chemoleo]
Never Stop to Begin, and Never Begin to Stop...
Tolerance is good. But not with the intolerant! (Wilhelm Busch)
|
|
|
JohnWW
International Hazard
   
Posts: 2849
Registered: 27-7-2004
Location: New Zealand
Member Is Offline
Mood: No Mood
|
|
| Quote: | Originally posted by S.C. Wack
Check your books, John. McAlpine and Soule:
"PbO2...is formed...(b) by treating Pb(II) in alkaline soln with oxidation agents, as halogens, H2O2, KMnO4, NaOCl, etc."
EDIT: Hawley's: "PbO2...Derivation: By adding bleaching powder to an alkaline solution of lead hydroxide."
Merck: "PbO2...Lab prepn from Pb(II) acetate and Ca(OCl)2: Newell, Maxson, Inorg Syn 1, 45 (1939)"
[Edited on 18-8-2004 by S.C. Wack] |
McAlpine and Soule are definitely WRONG about KMnO4 oxidizing Pb(II) to PbO2 in alkaline solution. As for H2O2, I suspect they are wrong again,
because even small amounts of heavy metals merely catalyse the autodecomposition of H2O2 with the evolution of oxygen. At best, it would take an
enormous excess of H2O2. However, NaOCl and dissolved Cl2 can do it, though.
John W.
|
|
|