MnO2/Fe2O3 separation


I've isolated MnO<sub>2</sub> many times from battery dry electrolyte by dissolving the MnO<sub>2</sub> in strong HCl to MnCl<sub>2</sub> and reoxidising the Mn (+II) to Mn (+IV), as described in the relevant thread on this forum.

Now I've been experiencing problems with a pottery grade MnO2 that contains about 20 - 25 w% iron oxide(s), expressed as Fe<sub>2</sub>O<sub>3</sub>. I want to eliminate the iron.

I'm wondering if the Mn and Fe could be separated by other means, as the HCl route is messy and generates lots of Cl<sub>2</sub>.

I have 51 w% H<sub>2</sub>SO<sub>4</sub> and am wondering whether some selective leaching would allow the Fe to dissolve as sulfate, leaving the MnO<sub>2</sub> behind, without need to reoxidise or re-precipitate.

Anyone have experience or ideas about this? :)
View user's profile View All Posts By User
woelen
Super Administrator
*********




Posts: 7978
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 6-4-2008 at 13:01


I think you will have a hard time doing this selective leaching. Problem is that the particles, even if they are very small, only react at their surface. You might get some Fe out from the surface, but the Fe, deeper inside the particles is not reached at all. What ever method you use, you need to either melt, or completely dissolve the material, in order to get all Fe in solution (or melt).

An added problem with potteries grade material is that it most likely is calcined. This makes the material less reactive. I have some potteries Fe2O3 and this stuff is amazingly inert. Most likely your MnO2/Fe2O3 materia forms some mixed salt, with iron and manganese at regular places in a crystal lattice, and then you can speak of a (possibly non-stoichiometric) compound, and not simply a mix. First row transition metals are most noteworthy capable of forming all kinds of mixed oxides of indeterminate stoichiometry.

You could try to get the material in solution with your H2SO4, by adding Na2SO3 or NaHSO3. The sulphur dioxide, formed in this reaction will reduce the MnO2 to Mn(2+) and I expect it to reduce the Fe(3+) to Fe(2+) and then the iron and the manganese go into solution. In this way you have a mix with Mn(2+) and Fe(2+). Adding an oxidizer like Na2S2O8 will precipitate out MnO2, even in somewhat acidic solutions, and Fe(3+) will remain in solution. Unfortunately using H2O2 as oxidizer does not work. In acidic solution, H2O2 works as reductor for MnO2 and besides that, it is decomposed catalytically very easily with Mn around.

[Edited on 6-4-08 by woelen]




The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
chemrox
International Hazard
*****




Posts: 2961
Registered: 18-1-2007
Location: UTM
Member Is Offline

Mood: LaGrangian

[*] posted on 6-4-2008 at 17:57
mining method


Here's an old mining method where the Fe is precipitated and the Mn stays in solution. No experience with it so don't know about how messy it may be.

Maybe you could get the material in solution treat it with dry ice, precip the iron carbonate hit it with acid and recover the oxide

[Edited on 6-4-2008 by chemrox]

Attachment: Fe from Mn by carbonate.pdf (780kB)
This file has been downloaded 532 times





"When you let the dumbasses vote you end up with populism followed by autocracy and getting back is a bitch." Plato (sort of)
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 7-4-2008 at 05:51


Woelen:

Agreed on the inertia of pottery grade Fe2O3: mine is also remarkably resistant to dissolution in HCl, it appears to dissolve only in part.

But the pottery grade MnO2 did dissolve easily in 32 w% HCl, even when cold, similarly to battery electrolyte and the Fe present dissolved readily as well.

I was also thinking of trying to part reduce the MnO2 by prolonged high temperature glowing with an excess of carbon, this should reduce it to Mn3O4, perhaps even MnO.