Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: Making CaC2 using a DC welder
metalresearcher
National Hazard
****




Posts: 822
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 24-11-2018 at 12:45
Making CaC2 using a DC welder


I repeated an earlier esxperiment of making calcium carbide which succeeded.
I put some charcoal with CaO powder in a crucible and put two carbon rods attached to a 140A DC welder into it.
I let it run a few minutes, which resulted in a very bright pinkish light and after cooling, I got a few chunks of (impure) CaC2 from the crucible.
The reaction is CaO + 3C => CaC2 + CO. The carbide is formed in a liquid state at a temperature well above 2000 C which freezes when cooling.
Throwing the carbide in water results in lots of C2H2 gas.

Here a video:

https://www.metallab.net/jwplayer/video.php?v=L2NsaXBzL0VBRi...




View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 24-11-2018 at 13:16


I thought about trying it a few times but in the end, I just ordered it off ebay ─ not as satisfying maybe, but a lot less effort...

View user's profile View All Posts By User
Ubya
International Hazard
*****




Posts: 1247
Registered: 23-11-2017
Location: Rome-Italy
Member Is Offline

Mood: I'm a maddo scientisto!!!

[*] posted on 25-11-2018 at 04:36


is it possible to measure the acetylene formed and from that calculate how much calcium carbide was made from the strarting reagents (just to have an idea of the yield)




---------------------------------------------------------------------
feel free to correct my grammar, or any mistakes i make
---------------------------------------------------------------------
View user's profile View All Posts By User
Texium
Administrator
Thread Moved
29-11-2023 at 11:38
Varungh
Hazard to Self
**




Posts: 70
Registered: 23-6-2025
Location: India
Member Is Offline

Mood: Bad mood

[*] posted on 10-2-2026 at 23:29


>Was the apparatus covered with something ( the powder starts to burn if kept uncovered)
>what container did you use. Alumina would melt near the temperature reached.
>What was the approx yeild?
>And how did you connect the electrodes to the welder? Copper connections would melt.
View user's profile View All Posts By User