[*] posted on 24-7-2011 at 23:52
Reactions related to Copper??


Dear all,
We have swimming pool heaters, which have heat exchangers made up of copper which are frequently damaged due to either salt present excessively or chlorine present excessively in the pool.

I need equations related to both the issues,

Can any one here give me reactions of hot Copper with salt water and chlorinated water.
View user's profile View All Posts By User
White Yeti
National Hazard
****




Posts: 816
Registered: 20-7-2011
Location: Asperger's spectrum
Member Is Offline

Mood: delocalized

[*] posted on 25-7-2011 at 10:35


Mind giving a little more info on what kind of corrosion is taking place?
Are you getting copper carbonate formation?
Is the copper reacting with oxygen to form CuO that washes away when water is pumped through the pipes?
Are you using ethylene glycol as a heat transfer fluid?
Are you getting pitting corrosion?

excuse me for answering a question with a question.
View user's profile View All Posts By User
Mr. Wizard
International Hazard
*****




Posts: 1042
Registered: 30-3-2003
Member Is Offline

Mood: No Mood

[*] posted on 25-7-2011 at 15:45


The very first thing I would suspect is electrolysis. Check to make sure the copper is not some part of a return or grounding connection with other electrical components. Make sure you use dielectric connectors when connecting this system to other piping. This is a known problem with water heaters.
View user's profile View All Posts By User
Mr. Wizard
International Hazard
*****




Posts: 1042
Registered: 30-3-2003
Member Is Offline

Mood: No Mood

[*] posted on 26-7-2011 at 12:57


Further thoughts on corrosion problem:
Where is the corrosion? Is it inside the pipe or outside? Is it near one end of the heat exchanger? The location of the corrosion will point to it's cause. Perhaps a sacrificial anode like used on boats or pipelines would help. They are cheap and safe. There is also an electronic version of the anode.

http://en.wikipedia.org/wiki/Sacrificial_anode