Perperation of calcium


The first method is the electroylsis of CaCl2, and KCl is used to lower the melting point.
But second method is a reduction method where Al powder is used to reduce its salt into pure calcium.
2 Al+3CaCl2=3Ca+2AlCl3
Aluminium chloride vaporizes at 180*C so I guess it can be boiled off leaveing the Ca behine.
But what will be required to start the reaction? Flame? Magnesium ribbon?




TNT
View user's profile View All Posts By User This user has MSN Messenger
Mumbles
Hazard to Others
***




Posts: 436
Registered: 12-3-2003
Location: US
Member Is Offline

Mood: Procrastinating

[*] posted on 25-4-2003 at 15:41


I don't know if that reaction would work. I think that you might need to use CaO. When the O is driven off it could be used to fuel the aluminum. I think an Oxidiser is a must in those reactions.
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
Polverone
Now celebrating 21 years of madness
*********




Posts: 3186
Registered: 19-5-2002
Location: The Sunny Pacific Northwest
Member Is Offline

Mood: Waiting for spring

[*] posted on 25-4-2003 at 16:01


The CaCl2 (or CaO) *is* the oxidizer. The calcium compound is reduced to the free metal, simultaneously oxidizing the aluminum to the corresponding compound (Al2O3 or AlCl3).

Metallic calcium is more electropositive than metallic aluminum, so I'm guessing that it's the higher lattice energy of the aluminum compounds that would drive this reaction.

Anybody care to confirm/deny my supposition?
View user's profile Visit user's homepage View All Posts By User
a_bab
Hazard to Others
***




Posts: 458
Registered: 15-9-2002
Member Is Offline

Mood: Angry !!!!!111111...2?!

[*] posted on 25-4-2003 at 22:45


Well, since C or even Fe are able to replace K or Na or Cs from their compounds, Al will obviously replace Ca. It's a matter ot temperature. To obtain K with iron around 1300 degrees C are needed.
I am researching now several methods to obtain Ca, Ba, Sr and for the Ca I guess I'll use the Moissan method one which will render pure Ca crystals. It's based on two facts: Ca is soluble in molten Na and Ca doesn't react with ethanol.

So, 600 grams of coarsely crushed anhydrous CaI2 are placed along with 250 grams of Na lumps (as large as a nut) in an iron crucible of 1 litre capacity. The crucible is closed with a screw lid and heated about an hour at a dull red heat then alowed to cool. The calcium which is soluble in excess of Na at red heat separates at the point of solidification and becomes practically insoluble. The metallic portion of the melt is cut-up into medium sized fragments and gradually introduced into absolute alcohol. The Na dissolves, leaving the Ca into brilliant white crystals (yummy !), 98.9 to 99.2 pc pure.

Well, I'll try the method along with several very exciting projcts when I'll have enough time and money and patience from my wife. The first project will be a "mini sodium factory" though...
View user's profile View All Posts By User
Nick F
Hazard to Others
***




Posts: 439
Registered: 7-9-2002
Member Is Offline

Mood: No Mood

[*] posted on 27-4-2003 at 03:27


The reaction of CaCl2 and Al will work due to the fact that AlCl3 is so volatile. It's an equilibrium reaction between Al + CaCl2 and AlCl3 + Ca, and the vapouristaion of AlCl3 forces the position of equilibrium towards Ca, giving a high yield. Lattice enthalpy probably plays a role too Polverone, since Al3+ is much smaller and more charged than Ca2+. But I think volatility of AlCl3 is the most important factor.
The same applies when using C or Fe as the reducing agent with metal oxides; CO2 escapes, leaving the metal, or with Fe, the metal is boiled off, leaving iron oxides.
View user's profile View All Posts By User
Polverone
Now celebrating 21 years of madness
*********




Posts: 3186
Registered: 19-5-2002
Location: The Sunny Pacific Northwest
Member Is Offline

Mood: Waiting for spring

[*] posted on 28-4-2003 at 08:41
ah, true


It would be interesting, then, to compare aluminothermic reduction of CaO vs. CaCl2, as Al2O3 is decidedly non-volatile.
View user's profile Visit user's homepage View All Posts By User
a123x
Hazard to Self
**




Posts: 87
Registered: 12-1-2003
Member Is Offline

Mood: No Mood

[*] posted on 11-5-2003 at 17:48


Anyone happen to know what type of temperatur is necessary to get Al to replace Ca+ in CaCl2? I came up with a rather simple set up to do this reaction with. Pretty much would just be a large L(except with the L rotated 90 degrees clockwise) shaped pipe with a valve located somewhere on the long part of the L. The CaCl2 + Al would be in the shorter part with the heat source under it, a vacuum cleaner would be attached to the open end of the long leg of the L to suck out forming AlCl3(g). When I feel the process is complete I would remove the heat and close the valve then let it cool down then remove my Ca.
View user's profile View All Posts By User
Theoretic
National Hazard
****




Posts: 776
Registered: 17-6-2003
Location: London, the Land of Sun, Summer and Snow
Member Is Offline

Mood: eating the souls of dust mites

[*] posted on 8-9-2003 at 06:24


Industrially, the Ca metal obtained by electrolysis is purified from salt impurities by passing (molten?) it over aluminium shavings. So I think it should work.:)
View user's profile View All Posts By User
kryss
Hazard to Self
**




Posts: 77
Registered: 11-7-2003
Location: N Ireland
Member Is Offline

Mood: No Mood

[*] posted on 9-9-2003 at 13:27


From Thermodynamics, data from
http://webbook.nist.gov/chemistry/

2Al +3CaCL2 -> 2AlCL3 + 3Ca
delta H = delta Hf(products-reactants)
=2x -706 - 3*(-796)
= -1412 +2384
= +1026 kj/Mol ie reaction strongly endothermic
2Al +3CaCL2 -> 2AlCL3 + 3Ca

At temp where AlCl3 is in gas phase:
S= 56+ 415 -> 628 + 123
delta S = 751-471= 280 j/molK ie
dG=dH-tdS where delta G=0
T= -1,026,000/ -280
T approx 3000 Kelvin for reaction to commence!
View user's profile View All Posts By User
Theoretic
National Hazard
****




Posts: 776
Registered: 17-6-2003
Location: London, the Land of Sun, Summer and Snow
Member Is Offline

Mood: eating the souls of dust mites

thumbdown.gif posted on 10-9-2003 at 04:50


Apparently NOT. If this reaction is used as a purification reaction, then it must be quite easy and simple to perform, and apparently at the temperature of the electrolysis bath (the temperature of calcium coming out of the electrolyser).;)
View user's profile View All Posts By User
ipr
Harmless
*




Posts: 1
Registered: 8-11-2003
Member Is Offline

Mood: ever

[*] posted on 8-11-2003 at 01:39


I had tried to melt Al with CaCl2 in air some time ago. There appear point flashes; I think these were Ca oxidizing in air. However no evidence of vaporing AlCl3 was observed.

I have found using phase diagram CaCl2-AlCl3 that the complex salt apparently arises preventing the evaporation of AlCl3. Duplex fluid is indicated only at high AlCl3 content. Maybe it is why no traces of reaction are observed?

There is a short reference to practical implementation of this reaction in the book by H.Remy. The reference is: Hackspill, 1951. However nothing in the kind was mentioned in Hackspill's Chimie Minerale.

Is there someone who knows Hackspill's original papers on preparation of calcium from CaCl2? Write me please.:(
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5105
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 8-11-2003 at 04:09


A couple of thoughts.
Why doesn't calcium react with alcohol? Mg does.
If the purification of calcium with aluminium is to remove other materials than the chloride then the reaction delta G would be different and the reation temperature might well be a lot lower.
I suspect the removal of oxide might be easier than chloride because you gain the lattice energy of the alumina (granted, you lose that of the CaO).
View user's profile View All Posts By User