Problem in making tungsten compounds
I have 11g of 99% tungsten wire, which is obtained from an old electronic store. For a long time I have been trying to convert the tungsten into its
compounds (WO3, WOCl4, WO2Cl2 or whatsoever), but have been unsuccessful.
I tried with direct burning it with a butane torch, the wire glows white upon heating, but it just became thinner as the atoms evaporate.
I have also tried to dissolve the metal by using aqua regia, conc hot HNO3, conc Sulphuric acid, but all these has no effect on the metal. I don't
have HF and don't want to buy it, but the metal also remains inert towards NH4HF2
So what should I do with the metal in order to obtain its compounds?
|
|
strontiumred
Harmless
Posts: 36
Registered: 6-7-2007
Location: Southern England
Member Is Offline
Mood: Delocalised
|
|
I think you need alkali and an oxidizing agent to make tungstate. Perhaps try adding dry sodium hydroxide with a nitrate or persulfate salt. Cover
the wire with this mixture then melt. I've not tried it with wire though, perhaps the surface area will not be enough?
Something like:
W + 3NaNO3 + 2NaOH --> Na2WO4 + 3NaNO2 + H2O
[Edited on 10-11-2011 by strontiumred]
|
|
IrC
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2710
Registered: 7-3-2005
Location: Eureka
Member Is Offline
Mood: Discovering
|
|
"Tungsten is a relatively inactive metal. It does not combine with oxygen at room temperatures. It does corrode (rust) at temperatures above 400°C
(700°F). It does not react very readily with acids, although it does dissolve in nitric acid or aqua regia."
From:
http://www.chemistryexplained.com/elements/T-Z/Tungsten.html
One would think you could take advantage of this rusting reaction, not to mention maybe your acid mix should be above room temperature if you use that
route. You might also search for making tungstic acid.
http://books.google.com/books/about/Experimenting_with_chemi...
To save you searching for the book Entropy51 mentions below. Also I did not know acids will not work, good to know but depressing to think you just
cannot trust anything on the web anymore. I liked that electrolysis idea. Can anyone provide more info such as chemicals used, as well as a good idea
of the proper voltages/currents, should the other electrode be carbon or Pt, etc., or another one of W?
[Edited on 11-11-2011 by IrC]
"Science is the belief in the ignorance of the experts" Richard Feynman
|
|
Endo
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 124
Registered: 5-1-2006
Location: USA
Member Is Offline
Mood: Cold
|
|
Acidified peroxide works, although it is slow it will chew up your tungsten over time. I dissolved several 1/4" round tungsten rod ends and discussed
the WO3 formation/ complex peroxytungstate ion formation in this post. Thanks to Not Important for his help on this.
http://www.sciencemadness.org/talk/viewthread.php?tid=6862#p...
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Nick F ![](images/xpblue/lastpost.gif) | Tungsten is easy to dissolve by electrolysis. I did this once to get the thoria out of some 2% thoriated electrodes. A search should bring up the
thread if you're interested. |
(from that thread)
|
|
entropy51
Gone, but not forgotten
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1612
Registered: 30-5-2009
Member Is Offline
Mood: Fissile
|
|
Tungsten is not attacked by acids. Tungsten powder will dissolve in boiling KOH solution to form the tungstate. The wire will not dissolve in
boiling KOH, rather it requires fusion with KOH or NaOH.
See page 55 of Experimenting with Chemistry: Experiments for the Home Lab By Burton L. Hawk which is available for free download on Google Books.
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by entropy51 ![](images/xpblue/lastpost.gif) | Tungsten is not attacked by acids. Tungsten powder will dissolve in boiling KOH solution to form the tungstate. The wire will not dissolve in
boiling KOH, rather it requires fusion with KOH or NaOH.
See page 55 of Experimenting with Chemistry: Experiments for the Home Lab By Burton L. Hawk which is available for free download on Google Books.
|
I found the book but not as a free download?
|
|
entropy51
Gone, but not forgotten
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1612
Registered: 30-5-2009
Member Is Offline
Mood: Fissile
|
|
On my screen there is a "PDF" button on the top right. I think
Google Books may limit downloads geographically so if your IP is not in the US it may not show for you.
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Yes, that may explain it. No free book for me then...
|
|
entropy51
Gone, but not forgotten
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1612
Registered: 30-5-2009
Member Is Offline
Mood: Fissile
|
|
Maybe Polverone would be kind enough to post this book in the forum library. It is one of the few available books on home
chemistry. I am only aware of five such books above the elementary school level. It would be nice if they were all in the library given the focus of
this forum.
|
|
LanthanumK
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 298
Registered: 20-5-2011
Location: New Jersey
Member Is Offline
Mood: No Mood
|
|
To make WO3 just pass a large amount of current through the filament. Anhydrous WO3 is formed, which undergoes hardly any reactions.
hibernating...
|
|
barley81
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 481
Registered: 9-5-2011
Member Is Offline
Mood: No Mood
|
|
In a previous thread, Woelen suggested electrolysis in alkaline peroxide to dissolve bulk tungsten. Here is the thread.
http://www.sciencemadness.org/talk/viewthread.php?tid=11962#...
|
|
LHcheM
Harmless
Posts: 37
Registered: 20-2-2011
Member Is Offline
Mood: No Mood
|
|
Well a long time since I logged on to this forum! I did put a wire into an acidified solution of hydrogen peroxide, I use quite a strong solution: 75%
H2SO4 with ~10% hydrogen peroxide, and the wire has become thinner since then...then problem is I didn't obtain a yellow precipitate of WO3, but
instead I got some light grey-black flakes in the solution? What's the possible reaction occurred?
I will try on the electrolysis later
|
|
nezza
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 324
Registered: 17-4-2011
Location: UK
Member Is Offline
Mood: phosphorescent
|
|
Tungsten can be oxidised, but needs rather severe conditions. I have made WO3 by adding tungsten as small pieces or powder to molten potassium and
sodium chlorate. It reacts fairly readily and burns red to white hot so a CLEAN pyrex tube can be used. The WO3 produced is insoluble in water or
acids, but can be dissolved in aqueous alkali. Be aware that molten chlorates are vigorous oxidising agents and will react violently with any traces
of organic material, hence the need for clean apparatus and pure salts.
|
|
careysub
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1339
Registered: 4-8-2014
Location: Coastal Sage Scrub Biome
Member Is Offline
Mood: Lowest quantum state
|
|
A bit of an old thread (2 years, 8 months since the last post) but I ran across an interesting ACS article about dissolving tungsten in 30% H2O2 and
nothing else:
http://pubs.acs.org/doi/abs/10.1021/ac60176a021
You can only read the first page without having an ACS login, but it pretty much covers the subject. They dissolved tungsten rod of various
thicknesses (fastest rate was at 60 C), time to complete dissolution:
5 mils, 1.5 hr
10 mils, 2.5 hr
15 mil, 2.75 hr
25 mil, 3 hr
If you plot this you see the time curve flattening out at 25 mil, so that the time for 60 mils (a 1/16" TIG electrode) would be a good bit less than
double the 25 mil time.
This would look like the method of choice for dissolving tungsten metal.
|
|
Polverone
Now celebrating 21 years of madness
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 3186
Registered: 19-5-2002
Location: The Sunny Pacific Northwest
Member Is Offline
Mood: Waiting for spring
|
|
Quote: Originally posted by careysub ![](images/xpblue/lastpost.gif) | A bit of an old thread (2 years, 8 months since the last post) but I ran across an interesting ACS article about dissolving tungsten in 30% H2O2 and
nothing else:
http://pubs.acs.org/doi/abs/10.1021/ac60176a021
You can only read the first page without having an ACS login, but it pretty much covers the subject. They dissolved tungsten rod of various
thicknesses (fastest rate was at 60 C), time to complete dissolution:
5 mils, 1.5 hr
10 mils, 2.5 hr
15 mil, 2.75 hr
25 mil, 3 hr
If you plot this you see the time curve flattening out at 25 mil, so that the time for 60 mils (a 1/16" TIG electrode) would be a good bit less than
double the 25 mil time.
This would look like the method of choice for dissolving tungsten metal.
|
Indeed. That's how I dissolved TIG rods.
PGP Key and corresponding e-mail address
|
|
jock88
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 505
Registered: 13-12-2012
Member Is Offline
Mood: No Mood
|
|
De page for posterity
|
|
careysub
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1339
Registered: 4-8-2014
Location: Coastal Sage Scrub Biome
Member Is Offline
Mood: Lowest quantum state
|
|
And it looks like a good way to separate the tungsten trioxide and thorium dioxide is to treat with NaOH and form the soluble sodium tungstate.
|
|
nezza
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 324
Registered: 17-4-2011
Location: UK
Member Is Offline
Mood: phosphorescent
|
|
Molten Potassium chlorate dissolves finely divided tungsten. I have tried it with crushed tungsten as smalll lumps/powder. The reaction is exothermic
so a pyrex tube is advisable and will need to be smashed to get at the mass of tungsten oxide once the reaction has stopped. It may work on tungsten
wire.
|
|