Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
 Pages:  1  ..  14    16    18  ..  24
Author: Subject: The trouble with neodymium...
Brain&Force
Hazard to Lanthanides
*****




Posts: 1302
Registered: 13-11-2013
Location: UW-Madison
Member Is Offline

Mood: Incommensurately modulated

[*] posted on 8-6-2014 at 12:04


It took you several tries? That's strange, because I was able to seperate terbium from the contaminated mixture in one go. But I had far less iron in solution than you had.

I have magnet soup of my own that I need to process.




At the end of the day, simulating atoms doesn't beat working with the real things...
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 8-6-2014 at 12:12


Personally I think it's possible to get the iron level down to almost 0 in one single purification, provided most of the iron is still in the ferrous state and you maintain high acidity all throughout the process.

But that's not really based on experience. When you precipitate the RE double sulphates from a sea of ferrous sulphate (Nd magnet soup), some co-precipitation of the FeSO4 may well be unavoidable...




View user's profile View All Posts By User
Brain&Force
Hazard to Lanthanides
*****




Posts: 1302
Registered: 13-11-2013
Location: UW-Madison
Member Is Offline

Mood: Incommensurately modulated

[*] posted on 8-6-2014 at 12:17


blogfast25, the differences in solubility between neodymium and terbium sulfates (terbium sulfate is far less soluble) may account for the observed differences. However, I need to find out exactly how much iron is needed to quench Tb fluorescence in order to set an upper limit on Fe contamination.



At the end of the day, simulating atoms doesn't beat working with the real things...
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 8-6-2014 at 13:04


Quote: Originally posted by Brain&Force  
blogfast25, the differences in solubility between neodymium and terbium sulfates (terbium sulfate is far less soluble) may account for the observed differences.


B&F, we're talking potassium Ln double sulphates here, not simple Ln (III) sulphates. I don't see how the solubility of the latter could influence the degree of separation from iron.




View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 8-6-2014 at 13:45


Quote: Originally posted by The Volatile Chemist  
Quote: Originally posted by MrHomeScientist  

It looks like I've finally been able to achieve effective separation of Fe and Nd!

Congradulations! Are you going to 'blog' about it? Or are there no pictures to show?


No photos of the process, sad to say. If I ever make it all the way to neodymium metal, there's absolutely a video in store when the process is perfected. It may be worthwhile to post one just getting the Nd separated (my progress up to this point).
View user's profile Visit user's homepage View All Posts By User
The Volatile Chemist
International Hazard
*****




Posts: 1981
Registered: 22-3-2014
Location: 'Stil' in the lab...
Member Is Offline

Mood: Copious

[*] posted on 8-6-2014 at 18:31


Quote: Originally posted by MrHomeScientist  
Quote: Originally posted by The Volatile Chemist  
Quote: Originally posted by MrHomeScientist  

It looks like I've finally been able to achieve effective separation of Fe and Nd!

Congradulations! Are you going to 'blog' about it? Or are there no pictures to show?


No photos of the process, sad to say. If I ever make it all the way to neodymium metal, there's absolutely a video in store when the process is perfected. It may be worthwhile to post one just getting the Nd separated (my progress up to this point).

Definitely would be a worthwhile post!




View user's profile Visit user's homepage View All Posts By User
Brain&Force
Hazard to Lanthanides
*****




Posts: 1302
Registered: 13-11-2013
Location: UW-Madison
Member Is Offline

Mood: Incommensurately modulated

[*] posted on 10-6-2014 at 14:43


I tried adding some potassium sulfate to my magnet nitrate mix, but barely any neodymium sulfate precipitated. After adding in some sulfuric acid to keep the pH up and halving the volume of the solution, still nothing precipitated. I then added some more potassium sulfate, and something did precipitate - and it redissolved after a few minutes! This neodymium does NOT want to leave solution, even after being subjected to yet another round of heating.

The concentration of all the iron and neodymium must be nearing 5 molar now, and that's a very conservative estimate. I don't have much time, nor can I keep the solution so I really might just have to dispose of the solution and use another magnet.

[edit] wait, there may be something I can do to save the solution...

[Edited on 10.6.2014 by Brain&Force]




At the end of the day, simulating atoms doesn't beat working with the real things...
View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 11-6-2014 at 06:42


Just an off the top of my head hypothesis, but mixing anoins might be "confusing" the precipitation. You could try dropping out everything as hydroxides, redissolving in sulfuric acid, and trying again to make the double sulfate. Perhaps in your case there just isn't enough sulfate around?

As for the earlier comment that it took me several tries, I think that was because of faulty method. Remember that I first started with "magnet sulfate" solution and added a saturated solution of K2SO4 to this. I got a good amount of precipitation, but this was heavily contaminated with iron due to, as blogfast pointed out, the addition of extra water changing the pH. I then returned this to solution and re-precipitated the double salt by directly adding solid K2SO4 instead of solution. This affords much, much cleaner precipitation. Comparing the leftover solution from the original precipitation with the leftover solution from the second method, it's clear that there's still some Nd left in the first one. So direct addition of the solid to the sulfate solution is definitely the way to go for effective and complete separation.

[Edited on 6-11-2014 by MrHomeScientist]
View user's profile Visit user's homepage View All Posts By User
Brain&Force
Hazard to Lanthanides
*****




Posts: 1302
Registered: 13-11-2013
Location: UW-Madison
Member Is Offline

Mood: Incommensurately modulated

[*] posted on 11-6-2014 at 14:22


That's a good idea with the multiple anion mixture, but the only thing I've been using to precipitate the neodymium are sulfates, and the only other anion in solution is nitrate - no hydroxides anywhere.

Also, I don't know if you've observed this, but whenever I heat the magnet nitrate solution, it turns very dark, but returns to its original color as it cools down. Is this because the nitrates are decomposing in solution?

Just wondering, where would be the best place to store a magnet nitrate solution for easy transport? It's quite acidic at this point, and I don't want to end my work now.




At the end of the day, simulating atoms doesn't beat working with the real things...
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 12-6-2014 at 04:39


Quote: Originally posted by Brain&Force  

Also, I don't know if you've observed this, but whenever I heat the magnet nitrate solution, it turns very dark, but returns to its original color as it cools down. Is this because the nitrates are decomposing in solution?



One possible explanation is the following. Using nitric acid as the acid to dissolve the magnets, the iron is oxidised to Fe<sup>3+</sup>. Ferric ion solutions are thermochromic because higher temperature pushes (simplified):

Fe<sup>3+</sup> + 2 H2O < === > Fe(OH)<sup>2+</sup> + H3O<sup>+</sup> to the right.

Fe(OH)<sup>2+</sup> is dark coloured in high concentrations (such as encountered in magnet soup). It appears this cation gives ferric solution it colour ranging from yellow to orange to much darker colours because [Fe(H<sub>2</sub>O)<sub>6</sub>]<sup>3+</sup> appears to be almost colourless.

[Edited on 12-6-2014 by blogfast25]




View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 12-6-2014 at 05:28


Quote: Originally posted by Brain&Force  
That's a good idea with the multiple anion mixture, but the only thing I've been using to precipitate the neodymium are sulfates, and the only other anion in solution is nitrate - no hydroxides anywhere.

What I meant was that you have a 'magnet nitrate' solution, and are adding sulfate to this. I have a 'magnet sulfate' solution, and am adding sulfate. So in my case there's more sulfate around, perhaps leading to easier precipitation. So my suggestion was to add hydroxide to precipitate everything, then redissolve in sulfuric acid instead.

Although now that I say that, blogfast has been working with 'magnet chloride' with no problems... hm.


As for the reversible color change, I've definitely noticed that too. It looks like some sort of thermochromism, not related to the anion (since ours are different). This experiment is full of surprises!
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 12-6-2014 at 09:56


Quote: Originally posted by MrHomeScientist  

Although now that I say that, blogfast has been working with 'magnet chloride' with no problems... hm.




It shouldn't matter what the main anion in the soup was: the moment you saturate it with K2SO4, the least soluble crystallites, i.e. the (Ln(III),K) double sulphates (as hydrates), crystallise out. Should also happen with nitrates present...




View user's profile View All Posts By User
Brain&Force
Hazard to Lanthanides
*****




Posts: 1302
Registered: 13-11-2013
Location: UW-Madison
Member Is Offline

Mood: Incommensurately modulated

[*] posted on 13-6-2014 at 07:54


I'm just spitballing here, but is it at all possible that a less soluble salt forms with the chloride along with the sulfate?



At the end of the day, simulating atoms doesn't beat working with the real things...
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 14-6-2014 at 05:14


Quote: Originally posted by Brain&Force  
I'm just spitballing here, but is it at all possible that a less soluble salt forms with the chloride along with the sulfate?


It's not impossible but we have no evidence for it. Better to stick with what we know.




View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 26-10-2014 at 14:48
Back on the Wagon


Once again I've come back to this project - this time attempting the final step: lithium reduction of neodymium fluoride.

3Li + NdF3 == 3LiF + Nd

For the impatient, it appears to have been a failure. The hot lithium most likely reacted with the air. Read on the for details.


For this first test, I used my first batch of the fluoride since it is very obviously contaminated by iron. It's green under fluorescent light, and pink in daylight.

NdF3.jpg - 167kB

After grinding to a fine powder, this was 1.4g NdF3. To this, I planned to react it with two slugs of my lithium, which was 0.17g.

Li slugs.jpg - 169kB

Molten lithium is very corrosive to a wide variety of materials, so choosing an appropriate crucible has proven to be difficult. I went with graphite this time, even though it is unsuitable for liquid lithium at 1000C (the target temperature here is 1024C, the melting point of Nd). I chose this because, frankly, it was what I had. Also I figure the lithium won't be around for very long at that temperature anyway, having mostly been reacted away by that time. Here's everything in the crucible.

Nd + Li in crucible.jpg - 166kB

I also did not use an inert atmosphere because, frankly, I haven't figured out the logistics of providing one to my crucible and furnace. I just wanted to try it out, and see if it did anything at all. Shortly after starting heating, the lithium started glowing red hot. You can see by the crucible that this is well under the temperature where this should be happening, so that must mean it reacted with something.

Li reaction.jpg - 191kB

After heating for several more minutes with no change, I put the crucible in my mini furnace and cranked it up to somewhere in the neighborhood of 1000C. Nothing ever melted.

Furnace.jpg - 239kB

After cooling, I was left with a rock hard mass of grey crust. This stuff is nearly impossible to remove from the crucible.

Li Nd Crust.jpg - 189kB

No metal of any kind in sight. It looks like the lithium reacted with the air first. I guess I'll need an inert blanket after all. I figured as much, but at least wanted to try this to see what happened.
View user's profile Visit user's homepage View All Posts By User
j_sum1
Administrator
********




Posts: 6241
Registered: 4-10-2014
Location: Unmoved
Member Is Offline

Mood: Organised

[*] posted on 26-10-2014 at 14:59


Great stuff -- well kinda.
Watching you closely since I intend to do much the same with LaCl3
(after buying some fluoride, after converting to LaF3, after crystallising, after purchasing a crucible, maybe after lining it with Mo or Ta, after building a furnace and after working out a way to feed argon into my setup...)
Right behind you.
View user's profile View All Posts By User
Tdep
National Hazard
****




Posts: 516
Registered: 31-1-2013
Location: Laser broken since Feb 2020 lol
Member Is Offline

Mood: PhD is done! It isn't good but it's over lol

[*] posted on 26-10-2014 at 16:11


This is such an interesting project.

I'm probably missing something, but can't you cover the reaction in sand or something similar? Surely that's a lot easier than building an inert atmosphere around it. Sure, you'll gets some silicon impurities from the lithium/SiO2 reaction but the molten Nd isn't going to reduce the sand is it? And if the NdF3 is layered above the lithium, the sand shouldn't get in the way that much. You're going to have to physically remove it, but you'll have to do that for the lithium slag anyway, even if a inert atmosphere is used.

If not sand, is there some other inert flux that will resist the high temperatures and the super reactive lithium? Aluminium oxide possibly??
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6241
Registered: 4-10-2014
Location: Unmoved
Member Is Offline

Mood: Organised

[*] posted on 26-10-2014 at 16:14


I had the same thought. But I was thinking excess NdF3. If the lithium was completely contained within a pile of the reactant then this would resolve some of the containment and side reaction issues.
View user's profile View All Posts By User
Pok
potassium Prometheus
***




Posts: 176
Registered: 5-12-2010
Member Is Offline


[*] posted on 26-10-2014 at 16:57


@MrHomeScientist: don't you think that neodymium itself will burn in air at such high temperatures? If any of it was produced by reduction with lithium, the product would look exactly the same (a mixture of lithium/neodymium oxide/fluoride).

Unfortunately, neodymium reacts with nitrogen when it burns (like lithium does). So if you can detect nitrides by reacting the product with water to produce ammonia, it would not necessarily mean that lithium reacted with air.

[Edited on 27-10-2014 by Pok]
View user's profile View All Posts By User
Zephyr
Hazard to Others
***




Posts: 341
Registered: 30-8-2013
Location: Seattle, WA
Member Is Offline


[*] posted on 26-10-2014 at 18:53


I recently made a small sample of neodymium sulfate by heating a magnet in concentrated sulfuric acid and then after letting the hot solution settle decanting off the top layer, and then repeating.
Here is the end product:




Sciencemadness Patches for sale! U2U me if you are interested.
http://imgur.com/a/QmpHn http://www.sciencemadness.org/talk/viewthread.php?tid=62566&...
View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 26-10-2014 at 19:25


Tdep: Molten lithium is some extremely corrosive stuff. We've been discussing it in a few other threads. The gist of it is that pretty much any oxide is no good, because the Li will rip the oxygen out of it. It reacts with glass pretty vigorously, so sand would be a no go. I'd definitely prefer inert blanket, if I can figure out how to do it.

Pok: Well the hope was that the LiF produced would form a protective layer over the denser Nd metal, if everything was good and molten. I charged the crucible by putting some of the NdF3 on the bottom, then the Li ingots, then covered with the rest of the fluoride. It might be better to put the Li on the bottom to better protect it and ensure the reaction goes from the bottom up, keeping the Nd buried and protected.
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 27-10-2014 at 05:55


Mr HS:

I think it could be useful to line the bottom of the crucible with a small excess of NdF3, to prevent the Nd metal sticking to the crucible. Just an idea...




View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 27-10-2014 at 09:01


Perhaps... I'm torn between using an excess of lithium (precious and reactive!) and using an excess of NdF3 (takes literally years for me to make! :) ).
In my other experiences with graphite crucibles, the stuff just pops right out. So I don't know - could be indication of a reaction between C and Li?

I thought a bit more about inert atmosphere today, and this is my preliminary idea for such a setup:

Inert Atmosphere Crucible.JPG - 50kB

A crucible (iron, graphite, Ta-lined, whatever) is placed inside an iron pipe with space around it. This space is filled with small steel ball bearings for heat transfer. An iron pipe cap is placed on top, with two holes drilled in it. Through these holes are inserted two smaller iron pipes for gas entry/exit.

Argon flows in from the left tube, which extends down into the crucible. It exits from the right tube, which only just comes in past the pipe cap. The entire assembly is heated from the outside via propane torch, and is expected to reach at minimum 1024C. (which is why copper won't work)

I have precisely zero experience working under these conditions, so if I have overlooked anything or if there is a severe safety hazard I'm missing please let me know.
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 27-10-2014 at 09:39


MrHS:

A small excess of NdF3 helps also as follows:

NdF3 + 3 Li < === > Nd + 3 LiF

... is pushed to the right. But use an excess Li instead and where will it end up?

Re. your argon design, perhaps using copper wire instead of ball bearings? But if you're heating from the bottom then neither may actually do all that much...




View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 27-10-2014 at 11:00


Well I wanted to avoid copper because the target temperature of Nd's melting point (1024C) is pretty close to copper's melting point (1085C). The last thing I want is a non-nuclear meltdown!

It might not be clear from picture 5, but my furnace has the torch come in from the side. Similar to picture 4. I figure I'll need to heat the whole thing up to 1024 to ensure molten products. I don't know if the reaction itself will proceed with heat to spare ala thermite.

Come to think of it, now that I have this furnace setup, is magnesium reduction a possibility again? We scrapped that because it didn't produce enough heat of reaction, but if I heat the whole thing externally that won't be a problem. Then I wouldn't need inert atmosphere either, which would simplify greatly. In fact I think I still have the Mg + NdF3 mixture that failed from my first attempt...
View user's profile Visit user's homepage View All Posts By User
 Pages:  1  ..  14    16    18  ..  24

  Go To Top