Author: Subject: Refining mercury from cinnabar
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 8-2-2012 at 13:56


Thanks for the idea!!! For 50g of cinnabar which size of test tube should I choose? ( I will buy this, since my cinnabar is pretty used....)

http://www.ebay.ca/itm/Powdered-Cinnabar-Crystal-50-g-Lot-Na...

[Edited on 8-2-2012 by plante1999]




I never asked for this.
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 9-2-2012 at 10:45


I used a 18*180mm test tube for the 20g amalgam batch, and I'd recommend this size.
I wouldn't try to react all 50g cinnabar at once- make a few smaller batches out of it, that way you won't lose everything if the test tube breaks, and you can improve your setup if it goes wrong the first time.

The test tube MUST be made of borosilicate glass (Pyrex,
Boro 3.3, Duran, or similar brands of borosilicate glass- mine was a Schott Duran test tube), the ordinary thin-walled soda-lime glass test tubes like Fiolax WILL break if you try to use them for this purpose! I've had that happen to me.

Borosilicate test tubes are somewhat difficult to shape by flameworking without an oxygen-fed burner due to their high softening point. It's a good sign if you can just barely get the test tube to soften with a bunsen burner on highest heat- this shows that you've got the right kind of glass. If the test tube softens very easily and you can even melt a hole in it, throw it away and buy some higher quality glass.





www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 9-2-2012 at 15:44


Does extra-fine steel wool will work as the iron source? For the test tube and heating it is ok. by the way , where did you get your dental amalgam?

Thanks alls for your help!




I never asked for this.
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 9-2-2012 at 20:23


I wouldn't use steel wool as the iron source, I'd think that proper mixing with the HgS could be a problem. You should get some fine iron filings first, or simply make them from a block of ordinary steel with a file.
However, you could put a little steel wool above the HgS + Fe mixture to react with any uncombined HgS vapor, and simultaneously act as a mechanical filter.

My surce of dental amalgams will remain confidential, and there's nothing more to be had. No dentist uses them any more anyway, so there's no source for any scraps.

[Edited on 10-2-2012 by garage chemist]




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 10-2-2012 at 04:53


Thanks for the help! It will be somewhat long to make 14g iron powder with a file.... Sorry I did not want to be impersonal about your dental amalgam. I have about 7-10g of cinnabar left from my experiments how could I make a Al/HgS battery? something like that but replacing the pyrite with cinnabar: http://www.youtube.com/watch?v=gu27nYYrM4w

Cinnabar is non conductive , so should I grind it to fine powder and ad really fine carbon powder for conductivity?




I never asked for this.
View user's profile View All Posts By User
Endimion17
International Hazard
*****




Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline

Mood: speeding through time at the rate of 1 second per second

[*] posted on 10-2-2012 at 08:48


Quote: Originally posted by plante1999  
...
by the way , where did you get your dental amalgam?

Thanks alls for your help!




:D




View user's profile Visit user's homepage View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 10-2-2012 at 10:12


Don't even think about asking a dentist for old amalgams that have been removed from patients teeth. These are held back in a gravity trap in the saliva suction device, and the stink from this sludge is unimaginable.
My amalgams were clean scraps from kneading the amalgam before inserting it into teeth. A fixed amount, e.g. 1g, of amalgam is prepared from a capsule containing alloy powder and liquid Hg, and the leftovers become rock hard after a short time, just like the filling itself.




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 10-2-2012 at 17:36


I finnaly made Mercury metal from cinnabar!!! I took 3g of HgS (cinnabar) which I aded to the end of a test tube, then I aded 1.3g of steel wool on top of the cinnabar which is a great exess. I aded a rubber stoper with a hole on the end of the test tube. I made a setup where the end of the test tube was in snow and I heated to brigth yellow the steel wool end with a propane torch. The mercury condensed as a miror where the snow was. I tapped the test tube in a steel beer cap. The mercury was not coalessing so I aded dilute HCl to coaless it and it worked! I got about 0.2ml of mercury. I cannot weight it since it is too small.


Thanks all for your Help and support!!!


<img src="http://i1103.photobucket.com/albums/g469/plante1999/Photo002-2.jpg" width="600" />

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: reduced image size(s)]

[Edited on 2.8.13 by bfesser]




I never asked for this.
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 11-2-2012 at 01:06


That's excellent to hear! Well done!
If you do this synthesis again, please make a picture of your setup before and after heating! I'd really like to see how the condensing mercury looks like when it is made from HgS + Fe instead of just being distilled from amalgams!
Also, please make a better picture of the mercury itself.
I'd also recommend that you redistill the mercury at least once when you have made somewhat more of it.




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
Endimion17
International Hazard
*****




Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline

Mood: speeding through time at the rate of 1 second per second

[*] posted on 11-2-2012 at 02:16


Please don't encourage him to distill mercury. You have no idea how dangerous that is.



View user's profile Visit user's homepage View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 11-2-2012 at 04:28


I will not redistill the mercury but I will make more from cinnabar ore. The next time I will make pictures. Im planning to react 62g of cinnabar in the next month which should give me about 4ml of mercury!! , this quantity is about what I need for making my own K,Na,Ce metal and then make hydroxide whith them. I am really happy with the results. So for making mercury from cinnabar you need steel wool, snow a test tube and stoper, propane torch and of course cinnabar.

(Now with my 0.2 ml I am making an amalgam with silver)

Thanks!

[Edited on 11-2-2012 by plante1999]




I never asked for this.
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 11-2-2012 at 05:53


If you don't redistill the mercury, at least filter it by pressing it through a cotton plug with a syringe. It is most likely seriously impure. At least mine from the amalgams was, it formed a thick dusty oxide layer during storage.

Distillation of the Hg is not necessarily more dangerous than the preparation from cinnabar and iron- after all, it doesn't make a difference whether you are heating liquid Hg or a mixture of HgS and Fe, the result is concentrated mercury vapor in both cases, and whether this is dangerous depends on your setup and technique.




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 11-2-2012 at 06:10


You can purify mercury to some extent by keeping it under dilute nitric acid, I seem to recall a lab procedure consisting of dripping contaminated Hg through a column of SG = 1.1 HNO<sub>3</sub>. The contaminant metals mostly dissolve in the nitric, leaving behind purified mercury.

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: subscript]

[Edited on 3.8.13 by bfesser]




View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 11-2-2012 at 06:17


In fact I purified my mercury from dilute (NH<sub>4</sub>;)<sub>2</sub>Cr<sub>2</sub>O<sub>7</sub> sol. and then i used it as a cathode in NaHCO<sub>3</sub> electrolite. I finnaly aded the mercury in distill water. It maked some effervessence, when the effervessence stoped the mercury was shining as a mirror, in fact I can see me on the droplet. this is a modified brauer process, brauer use KMnO<sub>4</sub>.

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: subscript]

[Edited on 3.8.13 by bfesser]




I never asked for this.
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 11-2-2012 at 09:32


On German Ebay there is a seller offering raw cinnabar ore rocks from Almaden, Spain by the kilogram:
http://www.ebay.de/itm/Zinnober-Almaden-Spanien-1-kg-verschi...
This is the stuff from which most of the mercury in use worldwide is being produced.
However, as the text states, this isn't pure cinnabar but rather the cinnabar-bearing rocks dug up from the ground in the mine.
I had a look in Ullmann's Encyclopedia under mercury and recent production figures from Almaden state that about 35kg of mercury are being produced from 1 metric ton of ore, e.g. the average mercury content of the ore is just 3,5%!
With 1kg of the ore costing EUR 25 plus shipping and only 35g mercury to be expected this is an expensive way to get mercury. Of course, 3,5% is just the average ore grade, this material could be a higher grade- ores from Almaden can reach 5-10% Hg and more.
Also, the large dilution of the HgS with rock means that the distillation with iron is not viable. Instead, the ore either has to be crushed and milled finely and the HgS enriched by flotation, or the crushed ore subjected to roasting with addition of air for the reaction that forms Hg and SO<sub>2</sub>.

The roasting process could be advantageously carried out in my tube furnace- a slow stream of air being pumped in by an aquarium membrane pump on one side, and the offgas led through a condenser to get the Hg.
I already have enough mercury for all my needs, so I don't need to do this, but it would be interesting nonetheless to find out how much mercury this ore contains so that other chemists who might be in need of mercury can decide for themselves whether they should make their own mercury from this material.
After all, metallic mercury is practically unavailable today except for tiny amounts from old thermometers.

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: subscript]

[Edited on 3.8.13 by bfesser]




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 11-2-2012 at 12:51


I tryed few way to make mercury from cinnabar.

Granular NaClO<sub>3</sub> + HgS: burn like flash powder when heated and release SO<sub>2</sub> + a wird gray-black coat that does not look like Hg

HgS + Air : just sublime the HgS... make a black coat of HgS.

Al + HgS : Make mercury that make black cinnabar, probably the hydrolisis of Al<sub>2</sub>S<sub>3</sub> make H<sub>2</sub>S

I tried them whith 0.1g of Cinnabar each.

[Edited on 11-2-2012 by plante1999]

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: subscript]

[Edited on 3.8.13 by bfesser]




I never asked for this.
View user's profile View All Posts By User
barbs09
Hazard to Others
***




Posts: 114
Registered: 22-1-2009
Location: Australia
Member Is Offline

Mood: No Mood

[*] posted on 12-2-2012 at 06:23


Hello, a slightly off topic but never-the-less related mercury question I would like to ask of the board: I have access to a good kg plus of mercury and would like the possibility of transporting it overseas to where I live. Shipping the liquid metal is out of the question for me, but I thought about amalgamating it with Zn powder and shipping (not aircraft) it as a plug of silver-grey coloured metal. Would this be considered a stable/inert enough form for shipping? Does anyone have any better ideas for rendering Hg more inert and passive for shipping purposes? Reacting with sulphur is also a possibility which would create material of cinnabar composition.

I am not interested in doing anything that would put anyone or any vessel at risk, nor myself in hot water.

Thoughts appreciated, Cheers ;)


View user's profile View All Posts By User
bfesser
Resident Wikipedian
*****




Posts: 2114
Registered: 29-1-2008
Member Is Offline

Mood: No Mood

[*] posted on 12-2-2012 at 06:49


Just a thought, but it may be easier and safer to just find a local source.



View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 12-2-2012 at 08:07


I dont think it is a great idee to ship 1kg of Hg over sea.... Dont even think to amalgamate it with Zn , The Zn release H<sub>2</sub> on contact with H<sub>2</sub>O when amalgamed.

Zn + H<sub>2</sub>O --> ZnO + H<sub>2</sub>

[Edited on 12-2-2012 by plante1999]

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: removed unnecessary quote; subscript; rxn. eqn. cleanup]

[Edited on 3.8.13 by bfesser]




I never asked for this.
View user's profile View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 12-2-2012 at 12:18


I made some mercury today from 9g of cinnabar and 5g of steel wool. here somme picture:

This is the set up

<img src="http://i1103.photobucket.com/albums/g469/plante1999/Photo004-2.jpg" width="600" />

I wanted to post a picture of the condensed mercury but the picture was realy black so I will not post it

Some picture of the mercury metal:


<img src="http://i1103.photobucket.com/albums/g469/plante1999/Photo008-1.jpg" width="600" />


<img src="http://i1103.photobucket.com/albums/g469/plante1999/Photo009-1.jpg" width="600" />

The reduction gave me 6g of mercury metal which is not bad.

In the futur weeks I will make more mercury, I hop the pictures will be betters.

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: reduced image size(s)]

[Edited on 2.8.13 by bfesser]




I never asked for this.
View user's profile View All Posts By User
Endimion17
International Hazard
*****




Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline

Mood: speeding through time at the rate of 1 second per second

[*] posted on 12-2-2012 at 13:03


Quote: Originally posted by plante1999  
...
So for making mercury from cinnabar you need steel wool, snow a test tube and stoper, propane torch and of course cinnabar.

(Now with my 0.2 ml I am making an amalgam with silver)

Thanks!

[Edited on 11-2-2012 by plante1999]


And a place to stay upwind.



Quote: Originally posted by garage chemist  
If you don't redistill the mercury, at least filter it by pressing it through a cotton plug with a syringe. It is most likely seriously impure. At least mine from the amalgams was, it formed a thick dusty oxide layer during storage.

Distillation of the Hg is not necessarily more dangerous than the preparation from cinnabar and iron- after all, it doesn't make a difference whether you are heating liquid Hg or a mixture of HgS and Fe, the result is concentrated mercury vapor in both cases, and whether this is dangerous depends on your setup and technique.


It is more dangerous because you have to heat the whole amount of mercury in the first tank which, if breaks, releases a stream of hot, gassing mercury. There's a video on YouTube where few guys try to distill it using an all glass apparatus. Unimaginable stupidity, on video!
Mercury is heavy, and boiling mercury, bumping, can shatter the apparatus. That simply must not happen because that would create a huge contamination of the whole room, enough for a serious hazmat scenario.

Of course, if one has steel equipment, pretty much all there is to worry about is the direction of wind.

Resonable purification can be done by agitating it few minutes with dilluted sulphuric and hydrochloric acid, leaving it overnight under the mixture, and then decanting with tap water. Next, metabisulphite bath to reduce any oxidized mercury in the disgusting layer covering the bulk metal. Short agitation with dilluted nitric acid can improve the purity. More goo could form, so again, metabisulphite bath, rinsing with tap water, then distilled water and drying with filter paper in the end.
I did that with my samples few years ago. They're stored in closed plastic containers. Still shiny. I've filled few instruments with it. No problems so far.



Quote: Originally posted by barbs09  
Hello, a slightly off topic but never-the-less related mercury question I would like to ask of the board: I have access to a good kg plus of mercury and would like the possibility of transporting it overseas to where I live. Shipping the liquid metal is out of the question for me, but I thought about amalgamating it with Zn powder and shipping (not aircraft) it as a plug of silver-grey coloured metal. Would this be considered a stable/inert enough form for shipping? Does anyone have any better ideas for rendering Hg more inert and passive for shipping purposes? Reacting with sulphur is also a possibility which would create material of cinnabar composition.

I am not interested in doing anything that would put anyone or any vessel at risk, nor myself in hot water.

Thoughts appreciated, Cheers ;)




That's around 3/4 of a decilitre. Why can't you ship it over the sea, using s ship? :)
It shouldn't be so expensive.



Quote: Originally posted by plante1999  
I made some mercury today from 9g of cinnabar and 5g of steel wool. here somme picture:

(...)



Here's an advice. Use macro on your camera. :)


Quote:
The synthesis gave me 6g of mercury metal which is not bad.

In the futur weeks I will make more mercury, I hop the pictures will be betters.


Analysis. It's impossible to chemically synthesize elements. ;)




View user's profile Visit user's homepage View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 12-2-2012 at 13:07


The word synthesis is Edited. Thanks for remmenbering me that!

[Edited on 12-2-2012 by plante1999]




I never asked for this.
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 12-2-2012 at 13:53


On the german forum, two members distilled 1kg mercury in an all-glass vacuum distillation setup, the kind that is used for general vacuum distillation of e.g. organic compounds.
This is not "unimaginable stupidity", but reasonably safe, just like vacuum distillation of other toxic compounds.
Boiling mercury does not bump. It boils smoothly even in vacuum, as these members have found out, and boiling capillaries are unnecessary.
I can search for the pictures if you want.




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
Endimion17
International Hazard
*****




Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline

Mood: speeding through time at the rate of 1 second per second

[*] posted on 12-2-2012 at 16:28


Mercury does bump at 1 atmosphere. I know because I've tried to boil it outside.

It is stupidity. Perhaps unimaginable is too harsh of a term, but it is very stupid.
I'm talking about this.
http://www.youtube.com/watch?v=PwbM5ZxVBzk
http://www.joshianlindsay.com/index.php?id=85
Almost 3.2 kilograms of mercury for each of three distillations.

Mercury boils at over 350 °C, which is perhaps exceeding the safe temperature for air condensers. But they use a Liebig condenser... filled with cooled water. They were extremely lucky, it could've bursted so easily. Liebig condensers with cold water aren't designed for such scenarios. Borosilicate glass shouldn't experience rapid temperature changes over the 150 degrees interval. Just imagine, their cooling water was probably lower than 10 °C, and mercury vapor is 356 °C. That introduces a lot of strain in the glass, and especially in its joints.

They didn't have any collecting plates beneath the apparatus. If the distillation flask had broken, the hot, boiling metal would flow through the heating mantle and spill over the table and on the floor. Just imagine what kind of contamination that is. It's horrifying!

Also, they keep a shitload of mercury in a regular glass reagent bottle. It's a rule to keep small amounts in bottles with thick glass walls, or in plastic bottles. Otherwise, the bottom can fall off.

And in the end, there's a ton of methanol in an open bowl, evaporating in the room. A real treat.

Now, if this isn't fucking stupid, I don't know what is.
Mercury is distilled in steel distillation systems.
Cinnabar is roasted in such systems, too.

I mean, come on, these are laboratory basics and common sense.
I didn't learn my chemistry from Youtube, but from books and practice and thinking "I might be wrong, let's see what smarter and older educated people think by checking in laboratory manuals".

Learning shit from Youtube introduces a lot more chance to learn something wrong, and Internet is not selective. Errors spread around.

[Edited on 13-2-2012 by Endimion17]

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: removed unnecessary quote(s)]

[Edited on 2.8.13 by bfesser]




View user's profile Visit user's homepage View All Posts By User
plante1999
International Hazard
*****




Posts: 1940
Registered: 27-12-2010
Member Is Offline

Mood: Mad as a hatter

[*] posted on 12-2-2012 at 16:54


I totally approuve this. This is why if someday I distill my mercury I will do it in steel welded pipe so there will be no leak and the steel is not suposed to break.

Edit: I will probably try this reaction:

4 CaCO<sub>3</sub> + 4 HgS --> 4 CO<sub>2</sub> + 3 CaS + CaSO<sub>4</sub> + 4 Hg

Calcium carbonate is easier to get than Iron powder...
This is a varient of a process that I saw in many documents.

[Edited on 13-2-2012 by plante1999]

<!-- bfesser_edit_tag -->[<a href="u2u.php?action=send&username=bfesser">bfesser</a>: removed unnecessary quote; rxn. eqn. cleanup]

[Edited on 3.8.13 by bfesser]




I never asked for this.
View user's profile View All Posts By User