[*] posted on 17-10-2012 at 20:46


Before you all get too carried away with the math... :D

Remember that chlorine, the product generated at the anode, is a gas and as such, impedes the reliable flow of current. Unfortunately, molten NaCl whose temperature range falls anywhere above NaCl MP and below Na BP is considerably viscous. I suppose this isn't such a big problem if the bath is heated externally in that the NaCl bath will remain molten regardless of the current density, etc.

In any case, once a certain anode current density is exceeded, a fearsome hiss will ensue and efficiency will go through the floor. This is actually an equilibrium between chlorine gas generation (and NaCl displacement from the anode) and the electrolyte flowing back to the anode (as chlorine bubbles off). The result is that the tip(s) of the anode(s) will carry more average current and will erode much faster than the superior part of the anode(s).

When the current density is decreased below that bitter sweet spot, I get 'burbling' at the anode. Sodium and chlorine are red/ox'ed rapidly. This is the Downs Cell sweet spot as far as I'm concerned.

Sorry, I got a bit off topic. Anyway, how does one account for gaseous product(s) when planning out electrode configuration, resistances, etc?? Surely the viscosity of the electrolyte must be taken into consideration??

Tank




Chemical CURIOSITY KILLED THE CATalyst.
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 18-10-2012 at 15:45


What's "considerably viscous"? My experience with molten salt has been a very watery consistency. Of course, I'm not about to mix water with it for a side-by-side test! :P



Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
m1tanker78
National Hazard
****




Posts: 685
Registered: 5-1-2011
Member Is Offline

Mood: No Mood

[*] posted on 18-10-2012 at 19:07


Quote: Originally posted by 12AX7  
...Of course, I'm not about to mix water with it for a side-by-side test! :P


I don't blame you! Anyway, I guess what I'm trying to say is that the residence time of chlorine on the anode must be taken into consideration when drafting equations and so forth... Or am I wrong? Even electrolysis in aqueous electrolyte tends to produce bubbles on electrode(s) that don't immediately rise to the surface. In most industrial settings where this is undesirable they usually incorporate vigorous stirring of some sort (as with electroplating). Yes, molten NaCl is watery but still not as free-flowing as water.

Tank




Chemical CURIOSITY KILLED THE CATalyst.
View user's profile View All Posts By User
WGTR
National Hazard
****




Posts: 972
Registered: 29-9-2013
Location: Online
Member Is Offline

Mood: Outline

[*] posted on 8-11-2013 at 18:41


Recently I did some experiments with molten salts, using my new electric furnace. This was basically just me "playing around"
with various salt mixtures, so sorry about being short on pictures this time around. I wanted to report these results, however,
because I thought some of them were interesting.

Using the information from this phase diagram here:
Li2CO3-Na2CO3.jpg - 78kB

I made a 50/50 mole% Li2CO3/Na2CO3 melt of about 17 grams total. The crucible was mild steel. I actually just wanted to
watch it melt, but once it did I decided to try electrolyzing it to see what would happen.

I figured that no alkali metals would form at the cathode, because for one thing, lithium is so reactive at those temperatures
that it would immediately react with the electrolyte if it was formed at all. So I used a copper wire as a cathode, and a graphite
rod as an anode, and electrolyzed the melt at 0.5-1.0A.

After running the cell for ten minutes or so, the power was shut off and the electrodes removed. The anode showed noticeable
erosion, but it was a "clean" erosion; it wasn't disintegrating or spalling, but wearing smoothly. The cathode was encased in a
hard, black, material that looked like carbon sponge. It was quite hard, but voluminous considering the amount of energy
that had passed through the cell. Upon submerging this cooled material in water, no gas evolution was noted. The black material
was then crushed underwater with pliers, and still no gas was produced.

Just for fun, I decided to add NaCl to the melt. After doing so, the molar composition of the molten bath was split evenly three
ways between NaCl, Li2CO3, and Na2CO3. Upon applying the same amount of current as before for about the same amount
of time, I noticed small "fireflys" appearing around the cathode. Tiny little orange flames would appear from time to time on
the surface of the electrolyte. No chlorine production was noted, although there was quite a bit of gas coming out from around
the anode. When the cathode was removed, the same hard black solid was present around the wire, but this time it reacted with
water, vigorously gassing for a couple of seconds. Every time the gas evolution slowed down, it could be restored by slightly
crushing the solid with pliers underwater. One time I had trouble breaking open a particularly hard piece, so I lifted it out of
water to crush it. Upon breaking open, the moist solid erupted into a 2cm yellow fireball, with a whisp of white smoke curling
away.

I tried the same experiment again, but this time with a copper anode that I had electroplated with nickel. The nickel was
suspended in the furnace exposed to the air for about an hour before it was submerged in the electrolyte. The results
at the cathode were the same. I was hoping that the anode erosion would be less, but it was inconclusive this time. The nickel
plating appearing to be loosening up, and I probably need to use a solid piece of nickel for this.

Afterward I was hunting around online to see if I could find some information that would corroborate what I had just done.
I think this is a relevant resource here, complete with pictures:

Attachment: 1209.3512.pdf (636kB)
This file has been downloaded 1737 times

In one case the electrolysis of molten Na2CO3/K2CO3 was noted as not leaving a coating of carbon on the cathode. Upon
adding Li2CO3, or CaCO3, a hard carbon deposit would begin to form at the cathode. As far as I know, no mention was made of
the presence or absence of alkali metals formed in any of their experiments.

As a result of my few tests, I'm not sure of the temperature at which Sodium reacts with a carbonate, but it appears that it can
coexist in the molten carbonate bath at about 650C....or at least it can when it is co-deposited into a solid conglomeration with
carbon.

View user's profile View All Posts By User
m1tanker78
National Hazard
****




Posts: 685
Registered: 5-1-2011
Member Is Offline

Mood: No Mood

[*] posted on 9-11-2013 at 06:38


WGTR:

There are a ton of side reactions that can (and do) take place in a cell of molten salt(s). Some of these are undocumented afaik. For me, the real fun was what I called 'garbage time'. When it came time to discard the fused salt mixtures, I always performed at least one experiment before shutting down the power.

Adding metal carbonates in almost any proportion drastically changes the cell reactions. You already observed the first and most obvious -- no (or very little) free chlorine gas is evolved. Your black sponge is sort of a glass-carbon-electrolyte-metal matrix. If you let it sit in air, it will develop some white spots that will become goop and then runny. Under some coercive conditions, one can make an intercalated solid this way.

Tank




Chemical CURIOSITY KILLED THE CATalyst.
View user's profile View All Posts By User
WGTR
National Hazard
****




Posts: 972
Registered: 29-9-2013
Location: Online
Member Is Offline

Mood: Outline

[*] posted on 9-11-2013 at 08:41


In a way this is what I'm going for: Intercalating (or alloying) alkali metals under cell conditions into a solid at the cathode.
This solid in turn will (hopefully) have similar reactivity to the pure alkali metal itself, while making it easier to collect the product.
The carbonate has a much lower decomposition potential at high temperatures than the equivalent chloride does. The oxide
requires even less. So really, no chlorine is formed unless one blasts the snot out of the anode.

The next experiment will probably start from this system:

NaCl-Na2CO3.jpg - 70kB

with Li2CO3 added incrementally until I begin obtaining an adherent deposit of carbon at the cathode. The current density was
probably too high for that little piece of wire last time, so I'll adjust it downward until sodium stops floating to the top of the bath.

Over time more carbonate will have to be added. In a way, CO2 is being co-electrolyzed using lithium as a catalyst
of sorts. According to the reference mentioned previously CaCO3 can be used to add CO2 back into the system, as CaCO3
is soluble in the melt, but the resulting CaO precipitates out.

Now, for a bit of fun with calcium I picked up some fluorspar (CaF2) from the pottery shop, and some CaCl2 from the grocery
store. The minimum melting point of this system is about 650C, which is much better than pure CaCl2 alone (772C). At 650C it
turns out that CaO is quite soluble in this melt, so this should allow me to avoid halogen gas production, as well as to use
a nickel/nickel oxide anode. Calcium metal is a solid at those temperatures, so its collection--especially at the lower melt
temperature--shouldn't be too difficult. I think at the melting point of CaCl2, calcium dissolves quite readily into the molten salt.
Anyway, if i get around to that, I'll post it in one of the "calcium" threads.
View user's profile View All Posts By User
m1tanker78
National Hazard
****




Posts: 685
Registered: 5-1-2011
Member Is Offline

Mood: No Mood

[*] posted on 9-11-2013 at 20:01


Quote: Originally posted by WGTR  

The carbonate has a much lower decomposition potential at high temperatures than the equivalent chloride does. The oxide requires even less. So really, no chlorine is formed unless one blasts the snot out of the anode.

The next experiment will probably start from this system:



with Li2CO3 added incrementally until I begin obtaining an adherent deposit of carbon at the cathode.
[...]
Over time more carbonate will have to be added. In a way, CO2 is being co-electrolyzed using lithium as a catalyst
of sorts. According to the reference mentioned previously CaCO3 can be used to add CO2 back into the system, as CaCO3
is soluble in the melt, but the resulting CaO precipitates out.

Now, for a bit of fun with calcium I picked up some fluorspar (CaF2) from the pottery shop, and some CaCl2 from the grocery
store. The minimum melting point of this system is about 650C, which is much better than pure CaCl2 alone (772C). At 650C it
turns out that CaO is quite soluble in this melt, so this should allow me to avoid halogen gas production, as well as to use
a nickel/nickel oxide anode. Calcium metal is a solid at those temperatures, so its collection--especially at the lower melt
temperature--shouldn't be too difficult. I think at the melting point of CaCl2, calcium dissolves quite readily into the molten salt.
Anyway, if i get around to that, I'll post it in one of the "calcium" threads.


Perhaps a 'molten salt experiments' thread should be opened?

If you want to recover your alkali metal(s) then forget about trying to form oxides. Oxide of any alkali/alkaline earth metal will spoil your experiment (the melt will freeze). With that in mind, carbonates are to be avoided as much as possible because they eventually decompose to oxide and greatly increase the needed heat input/current to keep the electrolyte molten. I've melted(!) a few carbon steel and stainless steel cathodes trying to 'fight the freeze' in the past.

Also, beware that a molten salt electrolyte that employs carbonate does produce some CO. I imagine highly toxic nickel carbonyl could easily form if one uses a nickel cathode under certain conditions.

A few 'typical' observations I made when sodium carbonate was included in the recipe:

One interesting side reaction I've observed is the formation of Fe3(CO)12 in a certain temperature range while the solid electrolyte is cooling. IIRC, I posted a pic in the 'pretty pictures' thread.

Warm sodium puts off an eerie blue flame in a CO2 atmosphere (i.e. decomposing sodium carbonate/bicarbonate). Sodium reduces CO2 to CO which in turn burns in air to produce a lovely blue flame. In slightly harsher conditions, sodium will reduce CO2 to carbon. Under very harsh conditions, sodium will reduce CO2 and form diamonds from the resultant carbon. I don't have the equipment to personally confirm that last one but I suppose you could just start with graphite. ;)

Sodium formate??? Affirmative.

Sodium hydride??? Maybe. Hard to prove and impossible for me to isolate from other salts. Evidence gives a nod but who knows?


A few scars and scares can be summed up with the following:

Safety should go beyond potential thermal burns and mass ejections of molten salt and alkali metal (been there!) :o I strongly recommend doubling up on eye protection. Goggles AND face mask should be worn even with small quantities. Some conditions favor emissions of toxic gasses and/or corrosive dust.

I can dig up some references if anyone is interested..

Tank




Chemical CURIOSITY KILLED THE CATalyst.
View user's profile View All Posts By User
WGTR
National Hazard
****




Posts: 972
Registered: 29-9-2013
Location: Online
Member Is Offline

Mood: Outline

[*] posted on 9-11-2013 at 23:19


I might move to a different thread if things really get off-topic, but not just yet.

I think that sodium will react with Na2CO3, I'm just not sure what temperature is required for that to happen. Lithium obviously
reacts with great vigor in the presence of carbonates at 650C. The melt consisting of Li2CO3 and Na2CO3 produced no
free alkali metal that I could notice. When NaCl was added, what I think happened is that the added concentration of Na+ in the
melt allowed sodium to start being reduced along with lithium at the cathode. The lithium reacted away, leaving some sodium
mixed in with the carbon. At least that's what I think, I could be wrong.

Certain oxides are actually soluble if the supporting electrolyte is compatible with them. Li2O and Na2O are fairly soluble in
this particular molten bath. CaO is much less so, but still soluble to a few percent or so. But yes, the way that I'm running this
bath will soon cause the electrolyte to solidify, due to depletion of carbonate, and the buildup of oxides. If CaCO3 is used
initially instead of Li2CO3, then the bath consists of CaCO3, Na2CO3, and NaCl. All of those salts are very cheap and easy to
find, so I don't think it would be a big deal to change out the electrolyte periodically.

In the case of the calcium system, the supporting electrolyte would be CaCl2/CaF2. The composition of that solvent shouldn't
change, since it wouldn't be electrolyzed. It would simply serve to dissolve a few percent of CaO, which would then be
electrolyzed. Extra CaO could be added as needed.

Certainly, if you have some references to share, I'd be happy to read through them. And I appreciate the discussion.

View user's profile View All Posts By User
Zyklon-A
International Hazard
*****




Posts: 1547
Registered: 26-11-2013
Member Is Offline

Mood: Fluorine radical

[*] posted on 26-11-2013 at 19:16


If considering chlorides, I suggest KCl, as it has a lower melting point, and potassium is more desired in my opinion.;)
View user's profile View All Posts By User
bfesser
Resident Wikipedian
Thread Pruned
26-11-2013 at 19:40
Metacelsus
International Hazard
*****




Posts: 2554
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline

Mood: Double, double, toil and trouble

[*] posted on 12-7-2015 at 11:34
NaK alloy production; shielding with wax


30g NaOH and 30g KOH were melted together in a 100 mL Ni crucible, then ~10A of current were passed through (voltage controlled with variac and rectifier to keep current more or less constant). Unfortunately, the metal burned off as soon as it formed.

Then, I realized that, because the temperature wasn't too high, I could melt paraffin wax on top of the hydroxide to exclude air. In this way, I obtained a pea-sized amount of NaK alloy, liquid at room temperature.

NaK metal.jpg - 126kB

[Edited on 12-7-2015 by Cheddite Cheese]




As below, so above.

My blog: https://denovo.substack.com
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 12-7-2015 at 11:40


Nice focus on your arm there, CC! ;)



View user's profile View All Posts By User
Metacelsus
International Hazard
*****




Posts: 2554
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline

Mood: Double, double, toil and trouble

[*] posted on 12-7-2015 at 12:46


https://youtu.be/anYM4eiJ6P8

A video of the electrolysis with no shielding. Note the sparks by the cathode.




As below, so above.

My blog: https://denovo.substack.com
View user's profile View All Posts By User
WGTR
National Hazard
****




Posts: 972
Registered: 29-9-2013
Location: Online
Member Is Offline

Mood: Outline

[*] posted on 13-7-2015 at 15:42


Quote: Originally posted by Cheddite Cheese  

Then, I realized that, because the temperature wasn't too high, I could melt paraffin wax on top of the hydroxide to exclude air. In this way, I obtained a pea-sized amount of NaK alloy, liquid at room temperature.

Very good job! That's an innovative and cheap solution to a difficult problem in lab-scale alkali metal production. If you
make another video using the paraffin approach, it would go right to my "download" folder.

View user's profile View All Posts By User
Metacelsus
International Hazard
*****




Posts: 2554
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline

Mood: Double, double, toil and trouble

[*] posted on 15-7-2015 at 10:43
Caution: wax is flammable!


I was doing another run, trying to make a good video (so I had my camera with me). A little bit of NaK must have come into contact with air despite the wax. It set the wax, which was heated past its flash point, on fire. I put it out by covering up the cell with a metal lid and waiting a few minutes for it to cool down.

wax fire.jpg - 7.2MB




As below, so above.

My blog: https://denovo.substack.com
View user's profile View All Posts By User
tsathoggua1
Hazard to Others
***




Posts: 335
Registered: 8-1-2017
Location: Beyond the pale
Member Is Offline

Mood: Phosphorescent

[*] posted on 4-4-2017 at 13:30


A couple of questions, if I may,

Of late, my father decided for some unfathomable reason to order some carbon crucibles. Why? I really don't know. Said he just wanted to play around with them, only, he's shown not the slightest sign of doing anything of the sort. Actually my suspicion is that he bought them expecting that I'd be the one using them (which he gave pernission to do) having realized that currently (pun intended) one of my latest projects is having yet another crack (or quite a lot of cracks, would be more like it, one after another after another after another, accompanied by plenty of flying molten sodium metal)

I have currently a power supply that will deliver either 14A@15V or 35A@5v and I've managed to make some Na and Na/Ca alloy with this, primarily using the higher amperage terminal of the power supply.

I've been concentrating on hydroxides as the melt, because of the reactivity issues with Cl2 salts, although adding a small amount of anhydrous CaCl2 to lower the melting point has been of use. And of course there is the issue of the intermetallic compound formed by fused hydroxide dissolving Na into it.

Now, the crucibles my old man ordered are of the black carbon type material, amorphous carbon AFAIK, I invested myself in some more crucibles of various kinds, steel/iron ones for plating in chromium or in nickel, I did treat myself to an all nickel crucible with lid through which a short length of glass or ceramic tubing will be inserted through the top as an insulating ring, not contacting the melt itself directly, but serving to merely insulate the incoming electrode wire(s) from the metal crucible body and lid.

The ones my old man bought are of the black, dense, quite hard carbon allotrope/polymorph, whilst one of the carbon ones I myself ordered is actual graphite, softer, silvery and unlike the black carbon type, which are reasonably difficult although not challengingly so to scratch with metal implements, the graphite ones are much softer, although the one that arrived today is perhaps a quarter inch thick.

Metal electrodes being used are either copper, or made out of a nickel alloy, the kind used for making guitar frets, since there is a large bucket chock full of fret-wire offcuts about 2'' long, and this alloy, whatever the composition, seems to stand up to fused NaOH very well, even when a blob of caustic is allowed to set on the end of one and that end, holding the other in pliers, is subjected to a roaring flame from a propane torch.

And whilst the black solid carbon (same stuff as is in battery carbon rods) crucibles seems to stand up to a fair lot of abuse, is there a significant difference in the resistance of this allotrope of carbon and of actual bona fide graphite per se, the true, softer (against indentation/scratching mechanically with hard metal or carbide tipped cutterss etc.) to fused alkali hydroxide melts at an equal degree of heat and time course, equal current/voltage and other variables, the variable changing being solely that of graphite vs black (non-vitreous) carbon?

And lastly, I seem to remember that a melt of NaOH and KOH, when fused, acts as an eutectic and in the right proportions, can result in the lowering of melting point of the mixed melt bath to as little as 200 degrees 'C.

Going to have a shot at preparing some NaK tonight now that today, Mr.Postie dropped off not only that large, thick graphite crucible but a nicely weighty sack of KOH, a few kg at least :)

What is the ideal eutectic proportion in an NaOH/KOH melt? and can it be further lowered with addition of a little anhydrous carbonate or bicarbonate?

Lastly, I have also potassium hydrogen phosphate. Two questions I have regarding this. Has it any role it may serve in the formulation of molten salt eutectics, and also, whether fused, or in aqueous solution, be reduced to phosphorous acid or hypophosphite salts? or for that matter, H3PO4 to these acids as is, without presence of counterion, since the presence of the hydrogen ion species should be sufficient to permit conductivity.
View user's profile View All Posts By User
Novichok
Harmless
*




Posts: 3
Registered: 15-7-2017
Member Is Offline

Mood: No Mood

smile.gif posted on 15-7-2017 at 02:13
Making sodium metal from sodium hidroxide


This process uses electrolysis as a means of synthesizing sodium metal. . . Using a heat-resistant vessel that does not conduct electricity, place sodium hydroxide in it and heat it to 320 degrees Celsius. When it reaches such temperature the compound will be liquid and therein place the positive and negative poles of the electrolysis cell and begin the process Of decomposition of the element, soon after a few hours will see white balls in one of the poles, this is the metal sodium, remove it from the container and put in a bowl with mineral oil and store, hopefully have helped. . . You may be confused by what I said, well I do not speak fluent English.:D

Na_sodium.jpg - 15kB
View user's profile View All Posts By User
Jstuyfzand
Hazard to Others
***




Posts: 166
Registered: 16-1-2016
Location: Netherlands
Member Is Offline

Mood: Learning, Sorta.

[*] posted on 15-7-2017 at 02:29


Congratulations! You just described the Castner process. :)
Although in practise it's a little more difficult.

[Edited on 15-7-2017 by Jstuyfzand]
View user's profile View All Posts By User
Novichok
Harmless
*




Posts: 3
Registered: 15-7-2017
Member Is Offline

Mood: No Mood

[*] posted on 15-7-2017 at 03:14
Making sodium metal from sodium chloride


This medium uses sodium chloride electrolysis. . . In a divided, heat-resistant container (between 1000 ° C) and that does not conduct electricity, place Sodium Chloride and warm the container above 800 degrees Celsius and below 850 Celsius, when heated place the positive and negative poles and when Once the electrolysis process is started, after a few hours there will be a chlorine smell, keep the place ventilated, the negative pole will have metallic sodium balls, separate them at the end of the process and place them in a pot with mineral oil
Attachment: phpOSLjs6 (33kB)
This file has been downloaded 1752 times

[Edited on 15-7-2017 by Novichok]
View user's profile View All Posts By User
gdflp
Super Moderator
Threads Merged
15-7-2017 at 06:26
gdflp
Super Moderator
Threads Merged
15-7-2017 at 06:26
Jstuyfzand
Hazard to Others
***




Posts: 166
Registered: 16-1-2016
Location: Netherlands
Member Is Offline

Mood: Learning, Sorta.

[*] posted on 13-8-2017 at 06:01


Would a mixture of NaOH and NaCl have a lower melting point than NaOH?
I could not find any papers or write ups about such mixture, which leaves me with low expectations, but it isnt disproven either.

If this mixture would have a lower temperature, it could be promising for Sodium production at home.
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 822
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 13-8-2017 at 09:12


Add CaCl2 to the NaCl and the mp will lower to 640 C.



View user's profile View All Posts By User
Jstuyfzand
Hazard to Others
***




Posts: 166
Registered: 16-1-2016
Location: Netherlands
Member Is Offline

Mood: Learning, Sorta.

[*] posted on 14-8-2017 at 06:10


Quote: Originally posted by metalresearcher  
Add CaCl2 to the NaCl and the mp will lower to 640 C.


I am aware of that, but 640 is still a bit high and unpractical.
A eutectic made with NaOH would be sub 330°C, so I was wondering whether a NaOH NaCl mixture would reach these lower temperatures.
View user's profile View All Posts By User
Bezaleel
Hazard to Others
***




Posts: 444
Registered: 28-2-2009
Member Is Offline

Mood: transitional

[*] posted on 24-11-2017 at 09:16


Quote: Originally posted by Jstuyfzand  
Quote: Originally posted by metalresearcher  
Add CaCl2 to the NaCl and the mp will lower to 640 C.


I am aware of that, but 640 is still a bit high and unpractical.
A eutectic made with NaOH would be sub 330°C, so I was wondering whether a NaOH NaCl mixture would reach these lower temperatures.

If you can tolerate the presence of potassium in your mixture, then consider the eutectic of NaCl, KCl, and CaCl2, which has a MP of 465 C. Check an earlier post here.